PVD (Physical Vapor Deposition) coating method based on Al material

By adopting a multi-layer film structure design on the surface of the aluminum alloy, including AlTi, AlTiC, pure Ti and TiAlSiC layers, the problems of binding force and corrosion resistance of aluminum alloy in PVD coating are solved, and the gradient transition of hardness and potential is achieved, which is significantly Improves the corrosion resistance and wear resistance of aluminum alloys.

CN118957493APending Publication Date: 2024-11-15TRITREE METAL SHENZHEN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411073413.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the PVD coating process, aluminum alloy materials have defects in binding due to the original oxide film and softness on the surface, and have poor corrosion and wear resistance.

Method used

Using a multi-layer film structure design, including AlTi layer, AlTiC layer, pure Ti layer and TiAlSiC layer, the hardness and potential gradient transition is achieved by adjusting the air pressure, power supply parameters and target configuration, and the load resistance and corrosion resistance of the film layer are enhanced. performance.

Benefits of technology

The corrosion resistance and wear resistance of the aluminum alloy surface are significantly improved, electrochemical corrosion between the film layers is avoided, hardness gradient transition is achieved, and the load resistance of the film layer is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957493A_ABST
    Figure CN118957493A_ABST
Patent Text Reader

Abstract

The invention discloses a PVD (Physical Vapor Deposition) coating method based on an Al material, and belongs to the field of PVD coating. Comprising the steps that S1, a substrate Al material is cleaned; s2, the coating chamber is heated and vacuumized; s3, argon is introduced, the air pressure reaches a preset value, bias voltage is set, and anode cleaning is conducted; s4, bias voltage is set, a medium-frequency coating power supply is turned on, meanwhile, Al and Ti target materials are turned on, and an AlTi layer is deposited; s5, C2H2 gas is introduced, meanwhile, the Al target and the Ti target are kept open, and an AlTiC layer is deposited; s6, the C2H2 gas is turned off, a medium-frequency Al target power source is turned off, the Ti target is kept to be turned on, and a pure Ti layer is deposited; and S7, the C2H2 gas is opened, meanwhile, the Al target, the Si target and the Ti target are opened, a TiAlSiC layer is deposited, and coating is finished. Compared with the prior art, by selecting elements of the base layer, the transition layer and the surface layer, hardness transition and potential transition between the layers are achieved, and it can be guaranteed that the film layer has excellent corrosion resistance; and hardness gradient transition can be reasonably achieved, and the loading resistance of the surface of the film layer is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of PVD coating, and in particular relates to a PVD coating method based on Al material. Background Art

[0002] Aluminum alloy materials have attracted much attention due to their low density, low price and excellent mechanical properties. In order to reduce the weight of electronic products such as mobile phones, watches, and headphones, various 3C manufacturers have gradually tended to choose aluminum alloys. However, since the surface of aluminum alloy has a loose oxide film, when PVD coating is performed, the bonding force between the PVD film and the substrate will be defective; in addition, since the aluminum alloy substrate itself is relatively soft, the high-energy bombardment of PVD will cause secondary defects on its surface. Therefore, direct PVD coating on the surface of aluminum alloy will show poor corrosion resistance, wear resistance and other properties. Summary of the invention

[0003] In order to solve the above problems, the purpose of the present invention is to provide a PVD coating method based on Al material, and the coated layer has corrosion resistance and wear resistance, thereby expanding the application scenarios of aluminum alloys.

[0004] To achieve the above object, the technical solution of the present invention is as follows:

[0005] The present invention provides a PVD coating method based on Al material, comprising the steps of:

[0006] S1: Cleaning the base Al material;

[0007] S2: placing the cleaned Al substrate into a coating chamber, heating and evacuating the coating chamber;

[0008] S3: When the local vacuum degree of the coating chamber reaches 0.001Pa, argon gas is introduced to make the gas pressure reach a predetermined value, the bias voltage is set, and the anode is cleaned;

[0009] S4: Adjust the argon gas intake to make the gas pressure reach a predetermined value, set the bias voltage, turn on the medium frequency coating power supply, and turn on the Al and Ti targets at the same time to deposit the AlTi layer;

[0010] S5: introducing C2H2 gas, adjusting the gas pressure, and keeping the Al and Ti targets turned on at the same time to deposit the AlTiC layer;

[0011] S6: Turn off the C2H2 gas, turn off the medium frequency Al target power supply, adjust the gas pressure to a predetermined value, keep the Ti target turned on, and deposit a pure Ti layer;

[0012] S7: Turn on the C2H2 gas, adjust the gas pressure to a predetermined value, turn on the Al, Si, and Ti targets at the same time, deposit the TiAlSiC layer multiple times, and end the coating;

[0013] Furthermore, in step S1, ultrasonic cleaning can remove dirt, fingerprints and other problems of the incoming base Al material, thereby ensuring the cleanliness of the base Al material before magnetron sputtering.

[0014] Furthermore, in step S2, the temperature of the coating chamber is 80-100°C.

[0015] Further, in step S3, the preset value of the gas pressure is 0.1 Pa, the bias voltage is -120 V, and the cleaning time is 900 s. In step S3, the base Al material is ion cleaned by anode glow, and after cleaning, the surface of the sample is flat and free of defects and impurities, which can achieve the surface cleaning effect within the range of minimum damage to the substrate, facilitating the implementation of the subsequent coating process.

[0016] Further, in step S4, the predetermined value of the gas pressure is 0.3 Pa, the bias voltage is set to -80 V, the deposition thickness of the film layer is 200-300 nm, the deposition time is 800-1200 s, the content of Ti in the film layer is 60%, and the content of Al is 40%.

[0017] Furthermore, in steps S4-S7, the current of the medium frequency coating power supply is 8A, the frequency is 40KHz, and the voltage is 500-800V.

[0018] In the present application, the design of the above power supply parameters can reduce the damage to the substrate during the film deposition process and control the temperature during the coating process; the gas pressure control can make the deposited film structure more in line with expectations and avoid grain growth defects.

[0019] Further, in step S5, after the gas pressure is adjusted to 0.31 Pa, the target material is opened for coating, the deposition thickness of the film layer is 300-500nm, the deposition time is 800-1200s, the content of Ti in the film layer is 54%, the content of Al is 36%, and the content of C is 10%.

[0020] Further, in step S6, the predetermined value of the gas pressure is 0.30 Pa, the deposition thickness of the film layer is 100-200 nm, and the deposition time is 600-1000 s.

[0021] Further, in step S7, the predetermined value of the gas pressure is 0.32 Pa, and the number of deposition times of the TiAlSiC layer is three times.

[0022] Furthermore, in step S7, the thickness of the TiAlSiC layer deposited for the first time is 400-500 nm, and the deposition time is 1500-2000 s, wherein the content of Ti in the film layer is 45%, the content of Al is 26%, the content of Si is 16%, and the content of C is 13%.

[0023] Furthermore, in step S7, the thickness of the TiAlSiC layer deposited for the second time is 300-400 nm, and the deposition time is 800-1200 s, wherein the content of Ti in the film layer is 37%, the content of Al is 18%, the content of Si is 26%, and the content of C is 19%.

[0024] Further, in step S7, the thickness of the TiAlSiC layer deposited for the third time is 200-300 nm, and the deposition time is 600-1200 s, wherein the content of Ti in the film layer is 44%, the content of Al is 10%, the content of Si is 26%, and the content of C is 20%.

[0025] In the present application, the nanohardness of the base Al material is generally about 4 GPa; the AlTi layer serves as the base layer, and its nanohardness is about 6 GPa; the AlTiC layer and the pure Ti layer serve as transition layers, and their hardness is about 9 GPa; the TiAlSiC layer serves as the surface layer, and its hardness is about 12 GPa. Through the stacking design of the above film layers, a reasonable hardness gradient transition can be achieved, and the loading resistance of the film surface can be effectively improved.

[0026] In addition, the electrode potential of aluminum is -1.663V, the electrode potential of Ti is -0.74V, the electrode potential of C is -0.1V, and the electrode potential of Si is 0.7711V. The elements of the base layer are Ti and Al, the elements of the transition layer are Ti, Al, and C, and the elements of the surface layer are Ti, Al, C, and Si. The Al element has a better affinity with the base Al material, and the potential is similar to the base Al material, which can achieve potential transition and avoid electrochemical corrosion caused by direct coverage of Ti by the aluminum substrate. At the same time, through the selection of elements in each layer, the potential of the base layer, transition layer, and surface layer can be gradually increased, so that the surface layer has better corrosion resistance, and the electrochemical corrosion caused by excessive potential difference between the film layers can be avoided.

[0027] Compared with the prior art, the beneficial effects of the present invention are as follows: the PVD coating method of the present application can achieve hardness transition and potential transition by selecting elements of the base layer, transition layer and surface layer, which can not only ensure that the film layer has excellent corrosion resistance and avoid electrochemical corrosion between layers; but also can reasonably achieve hardness gradient transition and effectively improve the loading resistance of the film surface. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a flowchart of the preparation method of this embodiment.

[0029] Figure 2 It is a film structure and composition diagram of the PVD film layer of this embodiment. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0031] To achieve the above object, the technical solution of the present invention is as follows:

[0032] See also Figure 1 As shown, this embodiment provides a PVD coating method based on Al material, the target material configuration includes a pair of Si targets, a pair of Al targets, a pair of Ti targets, and an anode, and the targets are all placed on the outside of the rotating frame (i.e., the furnace wall), wherein the Si target and the Al target are placed at the diagonal position of the equipment, and the two pairs of Ti targets are also placed diagonally, and the anode rod is placed on the inside of the rotating frame, and the coating method includes the following steps:

[0033] S1: Cleaning the base Al material;

[0034] S2: placing the cleaned Al substrate into a coating chamber, heating and evacuating the coating chamber;

[0035] S3: When the local vacuum degree of the coating chamber reaches 0.001Pa, argon gas is introduced to make the gas pressure reach a predetermined value, the bias voltage is set, and the anode is cleaned;

[0036] S4: Adjust the argon gas intake to make the gas pressure reach a predetermined value, set the bias voltage, turn on the medium frequency coating power supply, and turn on the Al and Ti targets at the same time to deposit the AlTi layer;

[0037] S5: introducing C2H2 gas, adjusting the gas pressure, and keeping the Al and Ti targets turned on at the same time to deposit the AlTiC layer;

[0038] S6: Turn off the C2H2 gas, turn off the medium frequency Al target power supply, adjust the gas pressure to a predetermined value, keep the Ti target turned on, and deposit a pure Ti layer;

[0039] S7: Turn on the C2H2 gas, adjust the gas pressure to a predetermined value, turn on the Al, Si, and Ti targets at the same time, deposit the TiAlSiC layer multiple times, and end the coating;

[0040] Furthermore, in step S1, ultrasonic cleaning can remove dirt, fingerprints and other problems of the incoming base Al material, thereby ensuring the cleanliness of the base Al material before magnetron sputtering.

[0041] Furthermore, in step S2, the temperature of the coating chamber is 80-100°C.

[0042] Further, in step S3, the preset value of the gas pressure is 0.1 Pa, the bias voltage is -120 V, and the cleaning time is 900 s. In step S3, the base Al material is ion cleaned by anode glow, and after cleaning, the surface of the sample is flat and free of defects and impurities, which can achieve the surface cleaning effect within the range of minimum damage to the substrate, facilitating the implementation of the subsequent coating process.

[0043] Further, see Figure 2 In step S4, the predetermined value of the gas pressure is 0.3 Pa, the bias voltage is set to -80 V, the deposition thickness of the film layer is 230 nm, the deposition time is 1000 s, the content of Ti in the film layer accounts for 60%, and the content of Al accounts for 40%.

[0044] Furthermore, in steps S4-S7, the current of the medium frequency coating power supply is 8A, the frequency is 40KHz, and the voltage is 500V.

[0045] In this embodiment, the design of the above power supply parameters can reduce damage to the substrate during film deposition and control the temperature during the coating process; gas pressure control can make the deposited film structure more in line with expectations and avoid grain growth defects.

[0046] Further, see Figure 2 In step S5, after the gas pressure is adjusted to 0.31 Pa, the target material is turned on for coating. The deposition thickness of the film layer is 300 nm, the deposition time is 800 s, the content of Ti in the film layer is 54%, the content of Al is 36%, and the content of C is 10%.

[0047] Further, see Figure 2 In step S6, the predetermined value of the gas pressure is 0.30 Pa, the deposition thickness of the film layer is 100 nm, and the deposition time is 600 s.

[0048] Further, see Figure 2 In step S7, the predetermined value of the gas pressure is 0.32 Pa, and the deposition times of the TiAlSiC layer is three times.

[0049] Further, see Figure 2 In step S7, the thickness of the TiAlSiC layer deposited for the first time is 480 nm, and the deposition time is 1700 s. In the film layer, the content of Ti is 45%, the content of Al is 26%, the content of Si is 16%, and the content of C is 13%.

[0050] Further, see Figure 2In step S7, the thickness of the TiAlSiC layer deposited for the second time is 300 nm, and the deposition time is 800 s. In the film layer, the content of Ti is 37%, the content of Al is 18%, the content of Si is 26%, and the content of C is 19%.

[0051] Further, see Figure 2 In step S7, the thickness of the TiAlSiC layer deposited for the third time is 200 nm, and the deposition time is 600 s. In the film layer, the content of Ti is 44%, the content of Al is 10%, the content of Si is 26%, and the content of C is 20%.

[0052] In this embodiment, the nanohardness of the base Al material is generally about 4 GPa; the AlTi layer serves as the base layer, and its nanohardness is about 6 GPa; the AlTiC layer and the pure Ti layer serve as transition layers, and their hardness is about 9 GPa; the TiAlSiC layer serves as the surface layer, and its hardness is about 12 GPa. Through the stacking design of the above film layers, a reasonable hardness gradient transition can be achieved, and the loading resistance of the film surface can be effectively improved.

[0053] In addition, the electrode potential of aluminum is -1.663V, the electrode potential of Ti is -0.74V, the electrode potential of C is -0.1V, and the electrode potential of Si is 0.7711V. The elements of the base layer are Ti and Al, the elements of the transition layer are Ti, Al, and C, and the elements of the surface layer are Ti, Al, C, and Si. The Al element has a better affinity with the base Al material, and the potential is similar to the base Al material, which can achieve potential transition and avoid electrochemical corrosion caused by direct coverage of Ti by the aluminum substrate. At the same time, through the selection of elements in each layer, the potential of the base layer, transition layer, and surface layer can be gradually increased, so that the surface layer has better corrosion resistance, and the electrochemical corrosion caused by excessive potential difference between the film layers can be avoided.

[0054] The performance test results of the film layer deposited in this embodiment are as follows:

[0055] 1. Corrosion resistance salt spray test: The corrosion resistance time of neutral salt spray is 48 hours; the corrosion resistance time of acid artificial sweat (pH4.7) is 48 hours; the corrosion resistance time of alkaline artificial sweat (pH9.5) is 48 hours;

[0056] 2. Hardness test: steel wool test (1Kg load) 3000 times; roller test 2 hours;

[0057] Roller test process:

[0058] 1. Before testing, make sure that there is no other medium in the drum except knives, keys and coins, including powdered substances. Knives, keys and coins should be replaced only when they are severely worn or damaged. When rolling, use polyimide tape to seal all open places of the assembly container;

[0059] 2. Before testing, inspect the product and record any appearance defects. Put the test product into a standard tumbler. Close the tumbler cover, tighten the nut and run the tumbler for 45 minutes;

[0060] 3. Take out the test sample and place it in the heavy medium modified tumbler, close the lid of the tumbler bucket, tighten the nut and run the modified tumbler for 15 minutes;

[0061] 4. Take out the test sample and clean it with a 50%-50% IPA-DI mixture and wet paper towels. If there is no obvious damage on the surface of the sample, it is qualified;

[0062] 5. After the test is completed, perform maintenance on the instrument as required.

[0063] The above test data show that the PVD film layer of this embodiment has excellent corrosion resistance and load resistance.

[0064] Compared with the prior art, the PVD coating method of this embodiment can achieve hardness transition and potential transition by selecting elements of the base layer, transition layer and surface layer, which can not only ensure that the film layer has excellent corrosion resistance and avoid electrochemical corrosion between layers; it can also reasonably achieve hardness gradient transition and effectively improve the loading resistance of the film surface.

[0065] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A PVD coating method based on Al material, characterized in that: Includes steps: S1: Cleaning the base Al material; S2: placing the cleaned Al substrate into a coating chamber, heating and evacuating the coating chamber; S3: When the local vacuum degree of the coating chamber reaches 0.001Pa, argon gas is introduced to make the gas pressure reach a predetermined value, the bias voltage is set, and the anode is cleaned; S4: Adjust the argon gas intake to make the gas pressure reach a predetermined value, set the bias voltage, turn on the medium frequency coating power supply, and turn on the Al and Ti targets at the same time to deposit the AlTi layer; S5: introducing C2H2 gas, adjusting the gas pressure, and keeping the Al and Ti targets turned on at the same time to deposit the AlTiC layer; S6: Turn off the C2H2 gas, turn off the medium frequency Al target power supply, adjust the gas pressure to a predetermined value, keep the Ti target turned on, and deposit a pure Ti layer; S7: Turn on the C2H2 gas, adjust the gas pressure to a predetermined value, turn on the Al, Si, and Ti targets at the same time, deposit the TiAlSiC layer multiple times, and end the coating.

2. A PVD coating method based on Al material as claimed in claim 1, characterized in that: In step S2, the temperature of the coating chamber is 80-100°C.

3. A PVD coating method based on Al material as claimed in claim 1, characterized in that: In step S3, the preset value of the gas pressure is 0.1 Pa, the bias voltage is -120 V, and the cleaning time is 900 s.

4. A PVD coating method based on Al material as claimed in claim 1, characterized in that: In step S4, the predetermined value of the gas pressure is 0.3 Pa, the bias voltage is set to -80 V, the deposition thickness of the film layer is 200-300 nm, the deposition time is 800-1200 s, the content of Ti in the film layer is 60%, and the content of Al is 40%.

5. A PVD coating method based on Al material as claimed in claim 1, characterized in that: In steps S4-S7, the current of the medium frequency coating power supply is 8A, the frequency is 40KHz, and the voltage is 500-800V.

6. A PVD coating method based on Al material as claimed in claim 1, characterized in that: In step S5, after the gas pressure is adjusted to 0.31 Pa, the target material is opened for coating, the deposition thickness of the film layer is 300-500nm, the deposition time is 800-1200s, the content of Ti in the film layer is 54%, the content of Al is 36%, and the content of C is 10%.

7. A PVD coating method based on Al material as claimed in claim 1, characterized in that: In step S6, the predetermined value of the gas pressure is 0.30 Pa, the deposition thickness of the film layer is 100-200 nm, and the deposition time is 600-1000 s.

8. A PVD coating method based on Al material as claimed in claim 1, characterized in that: In step S7, the predetermined value of the gas pressure is 0.32 Pa, and the number of deposition times of the TiAlSiC layer is three times.

9. A PVD coating method based on Al material as claimed in claim 1, characterized in that: In step S7, the thickness of the TiAlSiC layer deposited for the first time is 400-500 nm, and the deposition time is 1500-2000 s, wherein the content of Ti in the film layer accounts for 45%, the content of Al accounts for 26%, the content of Si accounts for 16%, and the content of C accounts for 13%; The thickness of the TiAlSiC layer deposited for the second time is 300-400 nm, and the deposition time is 800-1200 s. In the film layer, the content of Ti is 37%, the content of Al is 18%, the content of Si is 26%, and the content of C is 19%; The thickness of the TiAlSiC layer deposited for the third time is 200-300 nm, and the deposition time is 600-1200 s. In the film layer, the content of Ti is 44%, the content of Al is 10%, the content of Si is 26%, and the content of C is 20%.