Oxygen evolution electrode and preparation method and application thereof
Through ultrasonic synthesis method, the growth of nickel-iron-based metal alkoxide oxygen-excreting electrodes under normal temperature and pressure was solved, and the scale-up difficulty of nickel-iron-based metal alkoxide growth on current collectors in the prior art was solved, and high activity was achieved and stable electrode preparation, suitable for industrial applications of electrolyzed hydrogen production.
Patent Information
- Application Number
- CN202411015452.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-26
AI Technical Summary
In the prior art, the nickel-iron-based metal alkoxide is difficult to scale on the current collector, the growth conditions are harsh, the catalyst coverage is uneven and environmental pollution, which limits its large-scale industrialization in the production of hydrogen by electrolyzing water. application.
Using ultrasonic synthesis method, nickel nitrate, ferric nitrate, isopropanol and glycerol are mixed, and the current collector is ultrasonicated at normal temperature and pressure to achieve direct in-situ growth of nickel-iron-based metal alkoxide, and a high-active and stable oxygen evolution are prepared. electrode.
The oxygen-excitation electrode was successfully grown in a short time under normal temperature and pressure, which reduced the reaction activation energy, improved catalytic activity and stability. It was suitable for large-scale industrial production, simplified raw materials and processes, and was environmentally friendly.
Smart Images

Figure CN118957643A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrode catalysts, and in particular to an oxygen evolution electrode and a preparation method and application thereof. Background Art
[0002] Hydrogen has high energy density, is clean and green, and has a wide range of applications. It is gradually becoming one of the important carriers. How to efficiently and safely achieve hydrogen-to-electricity conversion is the core key to the green hydrogen energy industry. Among them, water electrolysis hydrogen production technology is the upstream part of the hydrogen energy industry, and its importance is rapidly increasing with the increase of renewable energy. At present, the mature and large-scale commercial electrolysis method for hydrogen production is alkaline water electrolysis technology. The oxygen evolution reaction (OER) in it has long been one of the biggest challenges facing this field due to its sluggish kinetics, difficulty in increasing current density, and long-term safety issues.
[0003] As the most efficient OER catalyst in alkaline electrolytes, nickel-iron-based catalysts have received extensive attention and made great progress. However, most of the current research on this type of catalyst is still at the laboratory scale, and the complex synthesis method and high cost limit the progress of its large-scale commercial application. The activity and stability of nickel-iron-based catalysts grown in situ on current collectors (such as nickel mesh, nickel felt or nickel foam) can meet the needs of industrial hydrogen production, but its preparation is currently mainly through water bath, electrodeposition or solvothermal methods, which have problems such as difficulty in scale-up, harsh growth conditions, uneven catalyst coverage and environmental pollution.
[0004] As an ideal alkaline OER catalyst, nickel-iron-based metal alkoxide catalysts can be easily converted into nickel-iron-based oxyhydroxides in situ during the electrolysis process. They are loose, amorphous, and rich in defects, which are very conducive to exposing active sites. However, the synthesis of nickel-iron-based metal alkoxides is still completely dependent on the solvothermal method, which requires high temperature, high pressure, and long-term synthesis conditions, and the prepared powder cannot be directly used as an electrode for water electrolysis. How to simply and efficiently grow nickel-iron-based metal alkoxides directly in situ on the current collector to provide the possibility for large-scale industrial hydrogen production is a key issue that needs to be solved urgently. Summary of the invention
[0005] The technical problem to be solved by the present invention is to overcome the defects of the prior art in which nickel-iron-based metal alkoxide is grown in situ on a current collector, such as the difficulty in scale-up, harsh growth conditions, uneven catalyst coverage and environmental pollution, and to provide an oxygen evolution electrode and a preparation method and application thereof. The oxygen evolution electrode exhibits high oxygen evolution reaction activity and good stability. The preparation method of the oxygen evolution electrode can not only directly grow nickel-iron-based metal alkoxide in situ on a current collector at room temperature and pressure in a short time to obtain an oxygen evolution electrode, but also has cheap raw materials, is environmentally friendly, and is suitable for industrial large-scale production.
[0006] The present invention discloses a method for preparing an oxygen evolution electrode, which comprises the following steps:
[0007] Mixing nickel nitrate, ferric nitrate, isopropyl alcohol and glycerol to obtain a mixed solution;
[0008] The current collector is placed in the mixed solution, and ultrasonicated at room temperature and pressure, wherein the frequency of the ultrasonication is 20 kHz-80 kHz, and the time of the ultrasonication is 2-10 h.
[0009] Preferably, the molar ratio of the nickel nitrate to the iron nitrate is (3-5):1.
[0010] Preferably, the nickel nitrate is nickel nitrate hexahydrate.
[0011] Preferably, the ferric nitrate is ferric nitrate nonahydrate.
[0012] Preferably, the concentration of the nickel nitrate is 80-240 mmol / L, measured in millimoles of nickel nitrate per liter of the total mixed solution.
[0013] Preferably, the concentration of the ferric nitrate is 30-50 mmol / L, measured in millimoles of the ferric nitrate contained in each liter of the total mixed solution.
[0014] Preferably, the volume ratio of the isopropanol to the glycerol is (10-30):1.
[0015] Preferably, the normal temperature is 15°C-40°C, for example 25°C.
[0016] Preferably, the normal pressure is 98 kPa-105 kPa, for example 101 kPa.
[0017] Further preferably, the molar ratio of the nickel nitrate to the iron nitrate is 4:1.
[0018] More preferably, the concentration of the nickel nitrate is 160 mmol / L, calculated on the basis of the millimolar amount of the nickel nitrate contained in each liter of the total amount of the mixed solution.
[0019] More preferably, the concentration of the ferric nitrate is 40 mmol / L, calculated as the millimole amount of the ferric nitrate contained in each liter of the total amount of the mixed solution.
[0020] More preferably, the amount of isopropanol used is 100-300 mL, for example 200 mL.
[0021] More preferably, the amount of glycerol used is 10-30 mL, such as 20 mL.
[0022] Preferably, the current collector is a nickel mesh, a nickel felt or a nickel foam, such as a nickel foam.
[0023] Preferably, the size of the current collector is 5 cm×5 cm.
[0024] Preferably, the pore density of the current collector is 75ppi-110ppi.
[0025] Preferably, the thickness of the current collector is 0.5-1.5 mm, for example 1 mm.
[0026] Preferably, the diameter of the pores of the oxygen evolution electrode is 100 μm-1000 μm.
[0027] In the present invention, the surface roughness of the current collector may be conventional in the art.
[0028] Preferably, the current collector is cleaned before the ultrasound.
[0029] Further preferably, the cleaning method is to place the current collector in acetone, hydrochloric acid, deionized water and anhydrous ethanol solutions for ultrasonic treatment respectively, and then take it out and dry it.
[0030] More preferably, in each solution, the ultrasonic time is 2-10 min, for example 5 min.
[0031] Preferably, the ultrasound is performed under a protective gas.
[0032] Further preferably, the protective gas is argon or nitrogen.
[0033] Preferably, the frequency of the ultrasound is 40kHz-80kHz.
[0034] Preferably, the ultrasonication time is 2-6 hours.
[0035] Preferably, after the ultrasound treatment, the current collector is rinsed and dried.
[0036] More preferably, the rinsing liquid is anhydrous ethanol.
[0037] Further preferably, the drying is carried out in a vacuum oven.
[0038] More preferably, the drying temperature is 50-70°C, such as 60°C.
[0039] More preferably, the drying time is 10-15 hours, such as 12 hours.
[0040] The invention also discloses an oxygen evolution electrode, which is prepared by adopting the preparation method of the oxygen evolution electrode.
[0041] The invention also discloses the application of the oxygen evolution electrode in producing hydrogen by electrolyzing water.
[0042] The positive and progressive effects of the present invention are:
[0043] (1) The ultrasonic synthesis method used in the oxygen evolution electrode of the present invention mainly utilizes the chemical energy provided by ultrasound. By adjusting the power of ultrasound to match the energy required for the change of chemical bonds in the chemical reaction process, the oxygen evolution electrode loaded with nickel-iron-based metal alkoxide can be prepared in a short time at room temperature and pressure. In addition, the preparation method is simple and feasible, the raw materials are cheap, and it is environmentally friendly. It is suitable for industrial large-scale production and can effectively promote the development of green hydrogen production technology.
[0044] (2) The oxygen evolution electrode of the present invention exhibits high oxygen evolution reaction activity and good stability. The oxygen evolution electrode prepared by the preparation method of the present invention is loaded with nickel-iron-based metal alkoxide, has good catalytic activity, reduces the reaction activation energy, and thus reduces the overpotential. The preferred embodiment of the present invention can achieve a current density of 500mA / cm at a voltage of 1.72V. 2 , and the overpotential is only 490mV. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 Schematic diagram of the experimental process of Example 1 and Example 2 of the present invention.
[0046] Figure 2 This is a scanning electron microscope image of the oxygen evolution electrode of Comparative Example 3 of the present invention.
[0047] Figure 3 This is a scanning electron microscope image of the oxygen evolution electrode of Example 1 of the present invention.
[0048] Figure 4 The oxygen evolution linear voltammetric curves of the oxygen evolution electrodes of Examples 1-3 of the present invention and Comparative Example 3 are shown.
[0049] Figure 5 This is the stability curve of the oxygen evolution electrode of Example 1 of the present invention. DETAILED DESCRIPTION
[0050] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples.
[0051] The reagents and raw materials used in the following examples, such as nickel nitrate hexahydrate and iron nitrate nonahydrate, are commercially available.
[0052] The nickel foam used in the following examples has a pore density of 110 ppi and a thickness of 1 mm.
[0053] Example 1
[0054] (1) Nickel nitrate hexahydrate and ferric nitrate nonahydrate in a molar ratio of 4:1 are dissolved in 200 mL of isopropanol, and 20 mL of glycerol is added to form a mixed solution. The concentration of nickel nitrate hexahydrate in the mixed solution is 160 mmol / L, and the concentration of ferric nitrate nonahydrate is 40 mmol / L.
[0055] (2) A nickel foam of 5 cm×5 cm in size was placed in acetone, hydrochloric acid, deionized water and anhydrous ethanol solutions, respectively, and ultrasonicated for 5 min in each solution. After being taken out, it was blown dry and then placed in the mixed solution of step (1) and continuously purged with nitrogen. The nickel foam was ultrasonicated continuously for 6 h at 40 kHz at a temperature of 25°C and a pressure of 101 kPa.
[0056] (3) The nickel foam after ultrasonic treatment in step (2) was taken out, rinsed with anhydrous ethanol, and placed in a 60° C. vacuum oven to dry for 12 h to obtain an oxygen evolution electrode.
[0057] Example 2
[0058] (1) Nickel nitrate hexahydrate and ferric nitrate nonahydrate in a molar ratio of 4:1 are dissolved in 200 mL of isopropanol, and 20 mL of glycerol is added. The concentration of nickel nitrate hexahydrate in the mixed solution is 160 mmol / L, and the concentration of ferric nitrate nonahydrate is 40 mmol / L.
[0059] (2) A nickel foam of 5 cm×5 cm was placed in acetone, hydrochloric acid, deionized water and anhydrous ethanol solutions for ultrasonic treatment, respectively. The foam was ultrasonicated for 5 min in each solution. After being taken out, it was blown dry and then placed in the mixed solution of step (1). Nitrogen was continuously purged and ultrasonicated at 20 kHz for 6 h at a temperature of 25°C and a pressure of 101 kPa.
[0060] (3) The nickel foam after ultrasonic treatment in step (2) was taken out, rinsed with anhydrous ethanol, and placed in a 60° C. vacuum oven to dry for 12 h to obtain an oxygen evolution electrode.
[0061] Example 3
[0062] (1) Nickel nitrate hexahydrate and ferric nitrate nonahydrate in a molar ratio of 4:1 are dissolved in 200 mL of isopropanol, and 20 mL of glycerol is added. The concentration of nickel nitrate hexahydrate in the mixed solution is 160 mmol / L, and the concentration of ferric nitrate nonahydrate is 40 mmol / L.
[0063] (2) A nickel foam of 5 cm × 5 cm was placed in acetone, hydrochloric acid, deionized water and anhydrous ethanol solutions for ultrasonic treatment, respectively. The foam was ultrasonicated for 5 min in each solution. After being taken out, it was blown dry and then placed in the mixed solution of step (1). Nitrogen was continuously purged and ultrasonicated at 40 kHz for 2 h at a temperature of 25°C and a pressure of 101 kPa.
[0064] (3) The nickel foam after ultrasonic treatment in step (2) was taken out, rinsed with anhydrous ethanol, and placed in a 60° C. vacuum oven to dry for 12 h to obtain an oxygen evolution electrode.
[0065] Comparative Example 1
[0066] After ultrasonic cleaning, the nickel foam of 5 cm×5 cm in size was taken out and placed in the mixed solution in step (1) of Example 1. The nickel foam was prepared by a hydrothermal method under the conditions of keeping the temperature at 160° C.-180° C. for 8-10 h.
[0067] Comparative Example 2
[0068] Other conditions were the same as those in Example 1, except that nickel nitrate hexahydrate and ferric nitrate nonahydrate in a molar ratio of 4:1 were dissolved in 220 mL of deionized water. It was found that an oxygen evolution electrode loaded with nickel-iron-based metal alkoxide could not be obtained.
[0069] Comparative Example 3
[0070] (1) Nickel nitrate hexahydrate and ferric nitrate nonahydrate in a molar ratio of 4:1 are dissolved in 200 mL of isopropanol, and 20 mL of glycerol is added to form a mixed solution. The concentration of nickel nitrate hexahydrate in the mixed solution is 160 mmol / L, and the concentration of ferric nitrate nonahydrate is 40 mmol / L.
[0071] (2) A nickel foam of 5 cm×5 cm in size was placed in acetone, hydrochloric acid, deionized water and anhydrous ethanol solutions, respectively, and ultrasonicated for 5 min in each solution. After being taken out, it was blown dry and then placed in the mixed solution of step (1) and continuously purged with nitrogen.
[0072] (3) The nickel foam after ultrasonic treatment in step (2) was taken out, rinsed with anhydrous ethanol, and placed in a 60° C. vacuum oven to dry for 12 h to obtain an oxygen evolution electrode.
[0073] The results showed that no substance was generated on the nickel foam substrate, and it was impossible to obtain an oxygen evolution electrode loaded with nickel-iron-based metal alkoxide.
[0074] Effect Example 1
[0075] Oxygen evolution reaction test:
[0076] The oxygen evolution reaction activity and stability of the oxygen evolution electrodes of Examples 1-3 and Comparative Example 3 were tested using a standard three-electrode system, the working electrode was the 1 cm×1 cm sample prepared above, the counter electrode was a platinum mesh, the reference electrode was Hg / HgO, the electrolyte was 1M KOH solution, and the electrochemical workstation used for the test was GAMRY Reference 3000.
[0077] The experimental process schematic diagram of Example 1 and Example 2 is as follows Figure 1 shown.
[0078] The scanning electron microscope image of the oxygen evolution electrode of Comparative Example 3 is as follows Figure 2 The surface morphology of the oxygen evolution electrode of Comparative Example 3 presents a pore structure of different sizes, the diameter of the pores ranges from 100 μm to 1000 μm, the surface is smooth, and there is no load.
[0079] The scanning electron microscope image of the oxygen evolution electrode of Example 1 is as follows Figure 3 The surface morphology of the oxygen evolution electrode of Example 1 presents a pore structure of varying sizes, with the diameter of the pores ranging from 100 μm to 1000 μm, and nickel-iron-based metal alkoxides are deposited or attached on the surface of the nickel foam and between the pores to form a uniform and rough covering.
[0080] The oxygen evolution linear voltammetric curves of the oxygen evolution electrodes of Examples 1-3 and Comparative Example 3 are as follows: Figure 4 It can be seen that the oxygen evolution electrode of Example 1 can reach a current density of 500 mA / cm when the voltage is 1.72 V compared with the reversible hydrogen electrode. 2 The theoretical potential of water electrolysis is 1.23V. In actual electrolysis, there is an overpotential, and the current density is 500mA / cm 2 The potential at the time is 1.72 V, and the overpotential is only 1.72 V-1.23 V = 0.49 V = 490 mV. The oxygen evolution electrodes of Examples 2 and 3 also exhibit certain oxygen evolution reaction activity, which is weaker than that of Example 1, but the activity of the untreated oxygen evolution electrode of Comparative Example 3 is significantly enhanced.
[0081] The stability curve of the oxygen evolution electrode of Example 1 is as follows Figure 5 The stability was evaluated by chronoamperometry at 300 mA / cm 2 At a current density of , the oxygen evolution electrode of Example 1 can operate stably for 100 hours.
[0082] Although the specific embodiments of the present invention are described above, it should be understood by those skilled in the art that this is only for illustration and the protection scope of the present invention is defined by the appended claims. Those skilled in the art may make various changes or modifications to these embodiments without departing from the principles and essence of the present invention, but these changes and modifications all fall within the protection scope of the present invention.
Claims
1. A method for preparing an oxygen evolution electrode, characterized in that: It includes the following steps: Mixing nickel nitrate, ferric nitrate, isopropyl alcohol and glycerol to obtain a mixed solution; The current collector is placed in the mixed solution, and ultrasonicated at room temperature and pressure, wherein the frequency of the ultrasonication is 20 kHz-80 kHz, and the time of the ultrasonication is 2-10 h.
2. The method for preparing an oxygen evolution electrode according to claim 1, characterized in that: The molar ratio of the nickel nitrate to the iron nitrate is (3-5):1; And / or, the nickel nitrate is nickel nitrate hexahydrate; And / or, the ferric nitrate is ferric nitrate nonahydrate; and / or, the concentration of the nickel nitrate is 80-240 mmol / L, measured in terms of the millimole amount of the nickel nitrate contained in each liter of the total mixed solution; and / or, the concentration of the ferric nitrate is 30-50 mmol / L, measured in terms of the millimole amount of the ferric nitrate contained in each liter of the total mixed solution; And / or, the volume ratio of the isopropanol to the glycerol is (10-30):1; And / or, the normal temperature is 15°C-40°C, for example 25°C; And / or, the normal pressure is 98 kPa-105 kPa, for example 101 kPa.
3. The method for preparing an oxygen evolution electrode according to claim 2, characterized in that: The molar ratio of the nickel nitrate to the iron nitrate is 4:1; and / or, the concentration of the nickel nitrate is 160 mmol / L, measured in terms of the millimolar amount of the nickel nitrate contained in each liter of the total amount of the mixed solution; and / or, the concentration of the ferric nitrate is 40 mmol / L, measured in terms of millimoles of the ferric nitrate contained in each liter of the total mixed solution; And / or, the amount of isopropanol is 100-300 mL, for example 200 mL; And / or, the amount of glycerol used is 10-30 mL, for example 20 mL.
4. The method for preparing an oxygen evolution electrode according to claim 1, characterized in that: The current collector is a nickel mesh, a nickel felt or a nickel foam, such as a nickel foam; And / or, the size of the current collector is 5 cm×5 cm; And / or, the pore density of the current collector is 75 ppi-110 ppi; And / or, the thickness of the current collector is 0.5-1.5 mm, for example 1 mm; And / or, the diameter of the pores of the oxygen evolution electrode is 100 μm-1000 μm.
5. The method for preparing an oxygen evolution electrode according to claim 1, characterized in that: The current collector is also cleaned before the ultrasound; Preferably, the cleaning method is to place the current collector in acetone, hydrochloric acid, deionized water and anhydrous ethanol solution for ultrasonic treatment, and then take it out and dry it; More preferably, in each solution, the ultrasonication time is 2-10 min, for example 5 min.
6. The method for preparing an oxygen evolution electrode according to claim 1, characterized in that: The ultrasound is performed under a protective gas; Preferably, the protective gas is argon or nitrogen; And / or, the frequency of the ultrasound is 40kHz-80kHz; And / or, the ultrasound duration is 2-6 hours.
7. The method for preparing an oxygen evolution electrode according to claim 1, characterized in that: After the ultrasound, the current collector is rinsed and dried.
8. The method for preparing an oxygen evolution electrode according to claim 7, characterized in that: The rinsing liquid is anhydrous ethanol; And / or, the drying is carried out in a vacuum oven; And / or, the drying temperature is 50-70°C, for example 60°C; And / or, the drying time is 10-15 hours, for example 12 hours.
9. An oxygen evolution electrode, characterized in that: The oxygen evolution electrode is prepared by the preparation method of the oxygen evolution electrode according to any one of claims 1 to 8.
10. Use of the oxygen evolution electrode as claimed in claim 9 in producing hydrogen by electrolysis of water.
Citation Information
Patent Citations
Ruthenium modified ferrocobalt hydroxide three-dimensional oxygen evolution electrode based on foam metal as well as preparation method and application of ruthenium modified ferrocobalt hydroxide three-dimensional oxygen evolution electrode
CN114959741A
Nickel-iron-based metal alkoxide catalyst as well as preparation method and application thereof
CN115896855A
Supported ferronickel-based oxygen evolution electrode and preparation method and application thereof
CN116180102A
Method for preparing self-supporting catalytic electrode through ultrasonic assistance and application of self-supporting catalytic electrode