Aperture-controllable hollow fiber film as well as preparation method and application thereof

The preparation of hollow fiber films with controllable pore sizes through electrospinning technology solves the problem of low sensitivity of piezoelectric fiber films, realizes high-performance acoustic and electrical detection, and demonstrates better electrical performance and environmentally friendly preparation technology.

CN118957876APending Publication Date: 2024-11-15SOUTHWEST JIAOTONG UNIV

Patent Information

Application Number
CN202410959319.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing piezoelectric fiber films have low sensitivity in mechanical wave monitoring and are difficult to control the pore size during preparation, which limits the acoustic wave capture capability.

Method used

Electrospinning technology is used to prepare hollow fiber films with controllable pore sizes. The precursor solution is formed by mixing PVDF, N-N dimethylacetamide, acetone and polyvinylpyrrolidone, and placed in a water bath to spin and then adjusting during annealing. The aperture achieves the formation of a hollow structure.

Benefits of technology

The sensitivity of piezoelectric fiber film is improved to reach 418.9mV/Pa, surpassing the performance of commercial piezoelectric films, and the preparation process is simple, the cost is low, and the material is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957876A_ABST
    Figure CN118957876A_ABST
Patent Text Reader

Abstract

The invention discloses an aperture-controllable hollow fiber film and a preparation method and application thereof, and belongs to the technical field of composite material preparation. According to the invention, PVDF is used as a basic shell layer material, PVP is used as a sacrificial layer core layer material, fiber films with different pore sizes are prepared by increasing the content of PVP in a core layer and combining coaxial electrostatic spinning, and controllability of the internal pore size of the fiber is realized. The fiber films with different apertures are stimulated at 50-1000Hz sweep frequency in a sound field, so that compared with solid fibers, the fibers with different apertures have an acoustoelectric enhancement effect, and have ultrahigh acoustoelectric sensitivity which can reach 418.9 mV / Pa to the maximum.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite material preparation, and in particular relates to a hollow fiber membrane with controllable pore size and a preparation method and application thereof. Background Art

[0002] In recent years, with the development and application of the era of big data intelligence, piezoelectric acoustics has been widely used in electronic equipment, information and sensing and other fields closely related to people's lives due to its self-powered and good linearity. However, due to the low pressure and large energy loss of sound waves during propagation, in order to make piezoelectric materials more sensitive to mechanical waves and improve the sensitivity of piezoelectric devices, it is necessary to further design piezoelectric materials. At present, piezoelectric materials are mainly inorganic piezoelectric ceramics (such as PZT) and polymers (such as PVDF). Inorganic piezoelectric ceramics have attracted widespread attention due to their high piezoelectric coefficients, but they are limited by the rigidity of the material itself; PVDF has the characteristics of simple and controllable operation process and low cost in polymers, and is widely used in various industries. However, in the monitoring of mechanical waves, the output response of PVDF film is not high, and its piezoelectric coefficient is about 30PC / N at most. The existing piezoelectric fiber film preparation is limited to disordered and completely ordered, and the piezoelectric output is still very low under the influence of sound waves, which makes the sensitivity of sound waves low. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a hollow fiber membrane with controllable pore size and a preparation method and application thereof, so as to solve the technical problem that the sensitivity of the piezoelectric fiber membrane is not high enough.

[0004] To achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing a hollow fiber membrane with controllable pore size, comprising the following steps:

[0005] S1. Mix PVDF, NN dimethylacetamide, acetone and polyvinyl pyrrolidone in a mass ratio of 1-2:3-4:1-2:0.5-1.5, and then heat in a water bath at 55-65°C for 25-35 minutes to obtain a precursor shell solution;

[0006] S2, polyvinyl pyrrolidone and anhydrous ethanol are mixed uniformly in a mass ratio of 0.5-1.5:4-6, and then heated in a water bath at 55-65° C. for 25-35 minutes to obtain a precursor core layer solution;

[0007] S3. Prepare a piezoelectric fiber film by electrostatic spinning the precursor shell layer solution and the precursor core layer solution, and then anneal the piezoelectric fiber film at 55-65° C. for 1.5-2.5 hours to obtain a hollow fiber film.

[0008] On the basis of the above technical solution, the present invention can also be improved as follows:

[0009] Furthermore, the mass ratio of PVDF, NN dimethylacetamide, acetone and polyvinyl pyrrolidone is 1.84:3.25:1.75:1.

[0010] Furthermore, the molecular weight of PVDF is 180,000 g / mol.

[0011] Furthermore, during the electrospinning process, the flow rates of the precursor shell solution and the precursor core solution were both 0.4-0.8 mL / h, the ambient temperature of the electrospinning was 20-30°C, the ambient humidity was 42-47%, the needle voltage was 14-16 kV, the spinning distance was 8-12 cm, and the spinning time was 1.5-2.5 h.

[0012] Furthermore, the annealing temperature is 60° C. and the annealing time is 2 h.

[0013] Furthermore, after annealing in step S3, the piezoelectric fiber film is placed in anhydrous ethanol and ultrasonicated for 1.5-2.5 hours.

[0014] Furthermore, the ultrasonic power is 150-180w.

[0015] The invention also discloses a hollow fiber membrane prepared by the preparation method.

[0016] The invention also discloses the application of the hollow fiber film in the preparation of piezoelectric acoustic devices.

[0017] The beneficial effects of the present invention are:

[0018] 1. The preparation process of the present invention is simple and easy to control. By adjusting different solution concentrations, the micro-nano adjustable hollow pore size can be achieved to meet different application requirements and realize the universality of hollow fiber application.

[0019] 2. The raw materials used in the present invention are polyvinylidene fluoride and polyvinyl pyrrolidone, which are low in cost and will not cause pollution to the environment.

[0020] 3. The present invention overcomes the problems of small strain and low output of traditional fibers. By controllably adjusting the different pore sizes of the fibers, the optimal pore size preparation (R2) is achieved. In the acoustic and electrical test, it exhibits excellent electrical performance, with a sensitivity of 418.9mV / Pa. In comparison with the commercial piezoelectric film test, it exhibits a lower distance (0.06), showing more excellent performance characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 is the fiber surface morphology;

[0022] Figure 2 The cross-sectional diagram of fibers with different pore sizes;

[0023] Figure 3 This is the analysis diagram of different fiber particle sizes;

[0024] Figure 4 This is a comparison and sensitivity test diagram of different structures in the sound field;

[0025] Figure 5 This is the sensitivity test chart at 90Hz;

[0026] Figure 6 Comparison of DTW distances between commercial membranes and hollow fiber membrane R2. DETAILED DESCRIPTION

[0027] The specific embodiments of the present invention are described below to facilitate the understanding of the present invention by those skilled in the art. If the specific conditions are not specified in the examples, the methods are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturers are not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially. However, it should be clear that the present invention is not limited to the scope of the specific embodiments. For those skilled in the art, as long as various changes are within the spirit and scope of the present invention defined and determined by the attached claims, these changes are obvious, and all inventions and creations using the concept of the present invention are protected.

[0028] Example 1

[0029] A method for preparing a hollow fiber membrane with controllable pore size comprises the following steps:

[0030] S1. Mix 1 g PVDF, 3 g NN-dimethylacetamide, 2 g acetone and 1 g polyvinyl pyrrolidone, and then heat in a water bath at 65°C for 35 min to obtain a bubble-free, transparent precursor shell solution.

[0031] S2, 1.5 g of polyvinyl pyrrolidone and 4 g of anhydrous ethanol were mixed evenly, and then heated in a water bath at 65° C. for 25 min to obtain a precursor core layer solution;

[0032] S3. The precursor shell layer solution is passed to the coaxial spinning outer layer of the electrospinning device, and the precursor core layer solution is passed to the coaxial spinning inner layer (the flow rate is 0.8 mL / h). The ambient temperature of the electrospinning is 20°C, the ambient humidity is 42%, the needle voltage is 16 kV, the spinning distance is 12 cm, and the spinning time is 1.5 h to obtain a piezoelectric fiber film. The piezoelectric fiber film is then annealed at 65°C for 1.5 h to remove the non-volatile solvent. Finally, the piezoelectric fiber film is attached to an acrylic plate, placed in anhydrous ethanol, and ultrasonicated at a power of 150 w for 2.5 h to dissolve the PVP in the fiber to obtain a hollow fiber film.

[0033] Example 2

[0034] A method for preparing a hollow fiber membrane with controllable pore size comprises the following steps:

[0035] S1. Mix 2 g PVDF, 4 g NN-dimethylacetamide, 1 g acetone and 1 g polyvinyl pyrrolidone, and then heat in a water bath at 55°C for 25 min to obtain a bubble-free, transparent precursor shell solution.

[0036] S2, 0.5 g of polyvinyl pyrrolidone and 6 g of anhydrous ethanol were mixed evenly, and then heated in a water bath at 55° C. for 35 min to obtain a precursor core layer solution;

[0037] S3. The precursor shell layer solution is passed to the coaxial spinning outer layer of the electrospinning device, and the precursor core layer solution is passed to the coaxial spinning inner layer (the flow rate is 0.4 mL / h). The ambient temperature of the electrospinning is 30°C, the ambient humidity is 47%, the needle voltage is 14 kV, the spinning distance is 8 cm, and the spinning time is 2.5 h to obtain a piezoelectric fiber film. The piezoelectric fiber film is then annealed at 55°C for 2.5 h to remove the non-volatile solvent. Finally, the piezoelectric fiber film is attached to an acrylic plate, placed in anhydrous ethanol, and ultrasonicated at a power of 180 w for 1.5 h to dissolve the PVP in the fiber to obtain a hollow fiber film.

[0038] Example 3

[0039] A method for preparing a hollow fiber membrane with controllable pore size comprises the following steps:

[0040] S1. 1.84 g PVDF, 3.25 g NN-dimethylacetamide, 1.75 g acetone and 1 g polyvinyl pyrrolidone were mixed evenly, and then heated in a water bath at 60°C for 30 min to obtain a bubble-free, transparent precursor shell solution;

[0041] S2, 1g of polyvinyl pyrrolidone (PVP) and 5g of anhydrous ethanol were mixed evenly, and then heated in a water bath at 60°C for 30min to obtain a precursor core layer solution;

[0042] S3. The precursor shell layer solution is passed to the coaxial spinning outer layer of the electrospinning device, and the precursor core layer solution is passed to the coaxial spinning inner layer (the flow rate is 0.6 mL / h). The ambient temperature of the electrospinning is 25°C, the ambient humidity is 45%, the needle voltage is 15 kV, the spinning distance is 10 cm, and the spinning time is 2 h to obtain a piezoelectric fiber film. The piezoelectric fiber film is then annealed at 60°C for 2 h to remove the non-volatile solvent. Finally, the piezoelectric fiber film is attached to an acrylic plate, placed in anhydrous ethanol, and ultrasonicated at a power of 160 w for 2 h to dissolve the PVP in the fiber to obtain a hollow fiber film (R2).

[0043] Example 4

[0044] The difference between this embodiment and embodiment 3 is that the polyvinyl pyrrolidone (PVP) in step S2 is replaced with 0.5 g, and the other implementation conditions are the same as those in embodiment 3, to obtain a hollow fiber membrane (R1).

[0045] Example 5

[0046] The difference between this embodiment and embodiment 3 is that the polyvinyl pyrrolidone (PVP) in step S2 is replaced with 1.5 g, and the other implementation conditions are the same as those in embodiment 3, to obtain a hollow fiber membrane (R3).

[0047] Comparative Example

[0048] The difference between this comparative example and Example 3 is that step S2 is omitted, and the precursor shell solution obtained in step S1 is subjected to electrostatic spinning and annealing to obtain a fiber film (R0).

[0049] Experimental Example 1 Structural Characterization

[0050] Figure 1 This is a SEM image of the hollow fiber membrane prepared in Example 3. It can be clearly seen from the image that the fibers are straight and uniform, without obvious beaded particles, proving that the prepared fiber membrane has good uniformity.

[0051] Figure 2 It is a cross-sectional view of hollow fiber membranes (R0-R3) with different PVP contents. It can be clearly seen from the figure that fibers with different PVP contents have different fiber pore sizes. As the mass fraction of the core layer PVP solution increases, the core layer inside the fiber also increases, thereby forming fiber membranes with different pore sizes.

[0052] Experimental Example 2 Particle Size Analysis

[0053] Figure 3It is a particle size analysis of fibers with different pore sizes, including the outer diameter and the internal pore size of the fiber. From the figure, it can be seen that the outer diameter of all fiber membranes is maintained at about 1.31-1.33μm, which further proves that the hollow fiber membrane prepared by the present invention has good uniformity. Through the analysis of the internal pore size of the fiber, it can be found that with the increase of PVP content, the internal pore size of the fiber increases from 0.3μm to 0.5μm, and finally reaches 0.9μm, realizing the controllability of the internal pore size of the fiber.

[0054] Experimental Example 3 Performance Analysis

[0055] The fiber membranes with different pore sizes (R0-R3) were stimulated with a sweep frequency of 50-1000 Hz in the acoustic field. Figure 4 and Figure 5 As shown, it can be seen that fibers with different pore sizes (R1-R3) have an acoustic-electric enhancement effect compared to solid fibers (R0), and have ultra-high acoustic-electric sensitivity, reaching up to 418.9 mV / Pa.

[0056] Figure 6 This is a comparison of the DTW distance (dimensionless) of the commercial membrane and the hollow fiber membrane R2. It can be seen from the figure that the test distance of the commercial sensor is 0.11, while that of R2 is 0.06, indicating that the signal measured by R2 is closer to the original signal, which further reflects that R2 has excellent electrical properties.

Claims

1. A method for preparing a hollow fiber membrane with controllable pore size, characterized in that: The following steps are involved: S1. Mix PVDF, NN dimethylacetamide, acetone and polyvinyl pyrrolidone in a mass ratio of 1-2:3-4:1-2:0.5-1.5, and then heat in a water bath at 55-65°C for 25-35 minutes to obtain a precursor shell solution; S2, polyvinyl pyrrolidone and anhydrous ethanol are mixed uniformly in a mass ratio of 0.5-1.5:4-6, and then heated in a water bath at 55-65° C. for 25-35 minutes to obtain a precursor core layer solution; S3. Prepare a piezoelectric fiber film by electrostatic spinning the precursor shell layer solution and the precursor core layer solution, and then anneal the piezoelectric fiber film at 55-65° C. for 1.5-2.5 hours to obtain a hollow fiber film.

2. The method for preparing a hollow fiber membrane with controllable pore size according to claim 1, characterized in that: The mass ratio of the PVDF, NN dimethylacetamide, acetone and polyvinyl pyrrolidone is 1.84:3.25:1.75:

1.

3. The method for preparing a hollow fiber membrane with controllable pore size according to claim 1, characterized in that: During the electrospinning process, the flow rates of the precursor shell solution and the precursor core solution are both 0.4-0.8 mL / h, the ambient temperature of the electrospinning is 20-30°C, the ambient humidity is 42-47%, the needle voltage is 14-16 kV, the spinning distance is 8-12 cm, and the spinning time is 1.5-2.5 h.

4. The method for preparing a hollow fiber membrane with controllable pore size according to claim 1, characterized in that: The annealing temperature is 60° C. and the annealing time is 2 h.

5. The method for preparing a hollow fiber membrane with controllable pore size according to claim 1, characterized in that: After annealing in step S3, the piezoelectric fiber film is placed in anhydrous ethanol and ultrasonicated for 1.5-2.5 hours.

6. The method for preparing a hollow fiber membrane with controllable pore size according to claim 5, characterized in that: The ultrasonic power is 150-180w.

7. A hollow fiber membrane with controllable pore size obtained by the preparation method according to any one of claims 1 to 6.

8. Use of the hollow fiber membrane according to claim 7 in the preparation of piezoelectric acoustic devices.

Citation Information

Patent Citations

  • Polymer-ceramic compound nanometer fibrous membrane as well as preparation method and application thereof

    CN102242464A

  • Core-shell fiber film material capable of spontaneously generating static electricity as well as preparation method and application of core-shell fiber film material

    CN117166137A

  • Polymer segregation film hydrophilization and biocompatibility modifying method

    CN1546214A

  • Polyvinyldenfluoride porous hollow fiber membrane and method for manufacturing same

    KR101380550B1

  • Nanofiber- and nanowhisker-based transfection platforms

    WO2021055939A1

Cited By

  • Swelling type hollow fiber container as well as preparation method and application thereof

    CN120443421A