Preparation method of elastic ceramic nanofiber membrane material
By introducing polymer heat shrink shape memory polymer and ceramic source components into ceramic materials, a multi-layer combined spinning technology is used to prepare a wrinkled ceramic nanofiber membrane, which solves the brittleness and rigidity of ceramic materials and realizes the ceramic materials Elastic transformation and high tensile strain capability have promoted its application in multiple fields.
Patent Information
- Application Number
- CN202411170353.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-26
AI Technical Summary
Due to its brittleness and rigid defects, ceramic materials have limited strain capacity and are difficult to meet the needs of complex deformation and impact loads, which limits their application in the fields of national defense and military industry, aerospace, flexible electronics, etc.
By mixing polymer heat-shrinkage shape memory polymer with ceramic source components, a ceramic nanofiber membrane with a wrinkled structure is prepared by using multi-layer combined spinning technology, and calcined in an inert or oxidative atmosphere to form an elastic ceramic nanofiber membrane. Overcome the brittleness problem of traditional ceramic materials.
It has achieved elastic transformation of ceramic materials, improved tensile resilience performance, and can meet the needs of complex deformation and impact loads, which is of great significance to the application of ceramic materials in many fields.
Smart Images

Figure CN118957885A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic nanofiber membranes, and in particular to a method for preparing an elastic ceramic nanofiber membrane. Background Art
[0002] Ceramic materials are widely used in aerospace, chemical, electronic and medical fields due to their excellent properties such as high temperature resistance, corrosion resistance, high strength and low density. However, due to the presence of defects such as dislocations, grain boundaries and rigid ionic / covalent bonds, ceramic materials usually show brittleness and rigidity. Compared with metals with high toughness or organic materials that can withstand large strains (5-100%), their strain capacity is often less than 1%, and they have poor operability, easy fracture when bent and deformed, and poor mechanical stability, which seriously restricts their actual application needs.
[0003] Due to the high aspect ratio and microstructural effect of nanofiber materials, the fiber network can bend, twist and slip when subjected to external forces, thus showing excellent deformation ability and flexibility under the action of external forces. Therefore, constructing fiberized ceramic materials from the nano or submicron scale is one of the effective ways to achieve the transformation of ceramic materials from brittle to flexible. The flexible ceramic nanofiber membrane obtained by nanofiberizing ceramic materials not only has the inherent characteristics of ceramic materials such as high temperature resistance, oxidation resistance, and corrosion resistance, but also has the excellent properties of fiber materials such as large aspect ratio, high flexibility and high porosity. Due to the wide variety of inorganic ceramic nanofiber materials, their preparation techniques are also diverse, currently mainly including chemical vapor deposition, electrospinning, centrifugal spinning and blow spinning.
[0004] However, with the development of emerging application fields such as wearable devices and high-temperature and high-frequency strain sensors, the limited tensile strain capacity of ceramic nanofiber membrane materials with single flexibility has made it difficult to cope with complex deformation and impact loads. Therefore, the development of ceramic nanofiber membrane materials with excellent flexibility, elasticity and high mechanical strength is of great significance to deepen the application of ceramic materials in defense and military industry, aerospace, flexible electronics, energy and environmental protection, biomedicine, personal protection and many other fields. Summary of the invention
[0005] In view of this, the present invention provides a method for preparing an elastic ceramic nanofiber membrane material, which can realize the preparation of an elastic ceramic nanofiber membrane material with a pleated structure. Its excellent tensile resilience can be widely used in national defense and military industry, aerospace, flexible electronics, energy and environmental protection, biomedicine, personal protection and other fields.
[0006] The object of the present invention is achieved through the following technical solution: a method for preparing an elastic ceramic nanofiber membrane material, the specific steps of which are as follows: S1, dissolving a high molecular weight heat shrinkable shape memory polymer in a solvent, and stirring evenly to obtain a polymer sacrificial template spinning solution A; S2, adding the ceramic source component into a certain hydrolysis system to prepare a precursor solution containing the ceramic source component, and then mixing the precursor solution with a spinning aid polymer solution, and stirring evenly to obtain a polymer / ceramic precursor solution B; S3, performing multi-layer combined spinning on solution A and solution B, peeling them off from the receiving substrate after a certain period of time, and then placing them in an oven at a certain temperature for a period of time to dry, thereby obtaining a multilayer ceramic precursor nanofiber membrane C; S4. calcining the obtained multilayer ceramic precursor nanofiber membrane C under a certain atmosphere for a period of time to prepare an elastic ceramic nanofiber membrane material.
[0007] Preferably, in S1, the polymer heat-shrinkable shape-memory polymer is at least one of polyurethane, polymethoxysilane, polyethylene, polystyrene, polyvinyl chloride, polypropylene, acrylonitrile-butadiene-styrene copolymer, styrene-butadiene-styrene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polydimethyl terephthalate, polybutylene terephthalate, polylactic acid, polyvinyl pyrrolidone, polycaprolactone, and polyoxymethylene; the solvent is at least one of water, anhydrous ethanol, isopropanol, acetone, N,N-dimethylformamide, dichloromethane, tetrahydrofuran, toluene, and acetylacetone, and the mass ratio of the polymer heat-shrinkable shape-memory polymer to the solvent is 1:3 to 1:13.
[0008] Preferably, in S2, the high molecular polymer is at least one of polyvinyl alcohol, polyvinyl butyral, polyvinyl pyrrolidone, polyethylene oxide, polyethylene glycol, and polyvinyl acetate; the solvent is at least one of water, anhydrous ethanol, isopropanol, acetone, N,N-dimethylformamide, dichloromethane, tetrahydrofuran, toluene, and acetylacetone, and the mass ratio of the high molecular polymer to the solvent is 1:1.5 to 1:9.
[0009] Preferably, in the S2, the ceramic source components are: the silicon source is tetramethoxysilane, tetraethoxysilane, tetraethyl orthosilicate, isopropyl orthosilicate; the zirconium source is zirconium acetate, zirconium chloride; the zinc source is zinc acetate, zinc nitrate; the tin source is tin acetate, tin chloride; the aluminum source is aluminum isopropoxide, aluminum sec-butoxide, aluminum chloride, aluminum nitrate, aluminum acetate; the titanium source is titanium trichloride, titanium tetrachloride, titanium oxysulfate, titanium acetylacetonate, isopropyl titanate, tetrabutyl titanate, tetraethyl titanate, diisopropoxy diacetylacetonate titanium; the barium source is carbonate Barium, barium acetate, barium sulfate, barium nitrate, barium chloride, barium hydroxide, barium oxide; lanthanum sources are lanthanum nitrate, lanthanum sulfate, lanthanum carbonate; lithium sources are lanthanum chloride, lithium nitrate, lithium sulfate, lithium chloride; silicon carbide source is polycarbosilane; the hydrolysis system is an acidic system or a neutral system, wherein the acidic substance corresponding to the acidic system is at least one of formic acid, acetic acid, oxalic acid, concentrated phosphoric acid, and concentrated hydrochloric acid, and the substance corresponding to the neutral system is water; the mass fraction of the hydrolysis system in the precursor solution containing the ceramic source components is 0.1% to 17%.
[0010] Preferably, in S3, the spinning technology includes at least one of electrospinning, blow spinning and centrifugal spinning, wherein the process parameters of the electrospinning process are: ambient temperature 20-35°C, humidity 10%-60%, injection speed 0.5-2mL / h, positive voltage 10-25kV, negative voltage 0.5-3.0kV, receiving distance 12-25cm, receiving speed 50-100r / min; the process parameters of the blow spinning process are: ambient temperature 20-35°C, humidity 10 %~60%, injection speed 1~15mL / h, blowing pressure 20~200kPa, blowing distance 5~80cm; the process parameters of the centrifugal spinning process are: ambient temperature 20~35℃, humidity 10%~60%, feed speed 0.1~20mL / h, spinning distance 5~30cm, spinneret speed 1000~20000rpm; the receiving substrate comprises at least one of silicone oil paper, release paper, non-woven fabric, tin foil, metal copper mesh, breathable cage and porous mesh curtain.
[0011] Preferably, in S3, the multi-layer combined spinning is one of a polymer / ceramic nanofiber double-layer membrane, a polymer / ceramic-polymer / ceramic nanofiber sandwich membrane, a polymer / ceramic / polymer nanofiber sandwich membrane, a polymer / ceramic-polymer / polymer nanofiber sandwich membrane, a ceramic / ceramic-polymer / polymer nanofiber sandwich membrane and a ceramic / polymer / ceramic nanofiber sandwich membrane combination structure; the drying temperature is 40-70°C, and the drying time is 6-24h.
[0012] Preferably, in S4, the calcination atmosphere is an inert atmosphere or an inert atmosphere converted to an oxidizing atmosphere, wherein the inert atmosphere is at least one of nitrogen and argon, and an elastic ceramic-carbon composite nanofiber membrane is obtained after calcination under an inert atmosphere; the oxidizing atmosphere is at least one of air and oxygen, and a pure inorganic elastic ceramic nanofiber membrane is obtained after calcination under an oxidizing atmosphere; the calcination temperature is gradually increased from room temperature to 500-1000°C, the heating rate is 0.5-10°C / min, and the insulation time is 0.5-8h.
[0013] Beneficial effects: The elastic ceramic nanofiber membrane prepared by the present invention adopts a shape memory polymer sacrificial template to induce the construction of the microscopic wrinkle structure of the ceramic nanofiber membrane, which overcomes the brittleness and rigidity defects of traditional ceramics, and realizes the performance transformation of the ceramic nanofiber membrane from "brittle" to "elastic", and by controlling the calcination atmosphere, elastic ceramic-carbon composite nanofiber membranes and pure inorganic elastic ceramic nanofiber membranes can be prepared; at the same time, the prepared stretchable elastic ceramic nanofiber membrane can meet the needs of complex deformation and impact load, which is of great significance to further promote the application of ceramic materials in national defense and military industry, aerospace, flexible electronics, energy and environmental protection, biomedicine, personal protection and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a physical picture of the silicon oxide elastic ceramic nanofiber membrane prepared in Example 2.
[0015] Figure 2 This is a laser confocal microscopy image of the silicon oxide elastic ceramic nanofiber membrane prepared in Example 2.
[0016] Figure 3 This is an electron microscope image of the silicon oxide elastic ceramic nanofiber membrane prepared in Example 2.
[0017] Figure 4 This is an electron microscope image of the wrinkle structure of the silicon oxide elastic ceramic nanofiber membrane prepared in Example 2.
[0018] Figure 5 This is a diagram of the cyclic tensile elastic properties of the silicon oxide elastic ceramic nanofiber membrane prepared in Example 2. DETAILED DESCRIPTION
[0019] The present invention will be further explained below in conjunction with the examples. The following examples are only used to illustrate the present invention, but are not intended to limit the scope of the present invention. Example 1
[0020] S1, dissolving the shape memory polymer polyvinylidene fluoride-hexafluoropropylene in a solvent of N,N-dimethylformamide and acetone (the mass ratio of the shape memory polymer to the solvent is 1:7), stirring at 400 r / min for 6 hours in a 40°C water bath to obtain a polymer sacrificial template spinning solution A; S2, adding 4.3g of tetraethoxysilane into an acidic hydrolysis system (the mass fraction of concentrated hydrochloric acid in the ceramic precursor solution is 0.3%) to prepare a silicon oxide ceramic precursor solution, which is then mixed with an aqueous solution of a spinning-aiding polymer polyvinyl alcohol (the mass ratio of the polymer to the solvent is 1:9), and stirred at 200r / min at room temperature for 1h to obtain a polymer / ceramic precursor (mass ratio of 7:3) solution B; S3, electrospinning the solution A and solution B in a combined layer of polymer / ceramic nanofiber double-layer membrane, under the conditions of humidity of 30±10% and temperature of 25±2°C, with silicone oil paper as the receiving substrate, the injection speed is set to 1mL / h, the receiving distance is set to 20cm, the receiving speed is 60r / min, the spinning voltage of the first layer solution A is +17kV / -1.2kV, the spinning voltage of the second layer solution B is +20kV / -1.3kV, the spinning time of each layer is 30min, and then it is peeled off from the silicone oil paper and placed in an oven at 70°C for 12h to obtain a polyvinylidene fluoride-hexafluoropropylene / silicon oxide ceramic nanofiber double-layer membrane C; S4. Place the shape memory polymer polyvinylidene fluoride-hexafluoropropylene / silicon oxide ceramic nanofiber double-layer membrane C in a tubular furnace, then heat it to 800°C at a heating rate of 1°C / min under a nitrogen atmosphere, keep it warm for 3 hours and then cool it naturally to obtain a silicon oxide elastic ceramic-carbon composite nanofiber membrane. Example 2
[0021] S1, dissolving shape memory polymer polystyrene in a solvent of N,N-dimethylformamide and tetrahydrofuran (the mass ratio of shape memory polymer to solvent is 1:3), stirring at 500 r / min for 6 hours at room temperature to obtain a polymer sacrificial template spinning solution A; S2, adding 4.3g of tetraethoxysilane into an acidic hydrolysis system (the mass fraction of concentrated hydrochloric acid in the ceramic precursor solution is 0.3%) to prepare a silicon oxide ceramic precursor solution, which is then mixed with an aqueous solution of a spinning-aiding polymer polyvinyl alcohol (the mass ratio of the polymer to the solvent is 1:9), and stirred at 200r / min at room temperature for 1h to obtain a polymer / ceramic precursor (mass ratio of 7:3) solution B; S3, electrospinning solution A and solution B in the form of a polymer / ceramic-polymer / ceramic nanofiber sandwich membrane, at a humidity of 20±10% and a temperature of 25±5°C, with silicone oil paper as the receiving substrate, the injection speed is set to 1 mL / h, the receiving distance is set to 20 cm, the receiving speed is 60 r / min, the spinning voltage of the first layer solution A is +20 kV / -3.0 kV, the spinning voltage of the second layer solution A and solution B is +20 kV / -1.3 kV, the spinning voltage of the third layer solution B is +20 kV / -1.3 kV, the spinning time of each layer is 30 min, then it is peeled off from the silicone oil paper and placed in an oven at 60°C for 24 h to obtain a polystyrene / silicon oxide-polystyrene / silicon oxide nanofiber sandwich membrane C; S4. Place the polystyrene / silicon oxide-polystyrene / silicon oxide nanofiber sandwich membrane C in a tubular furnace, then heat it to 800°C at a heating rate of 5°C / min in a nitrogen atmosphere, keep it warm for 3 hours, then switch to an air atmosphere, keep it warm for another 3 hours, then cool it down naturally to obtain a silicon oxide elastic ceramic nanofiber membrane.
[0022] As can be seen from the attached figure, a large number of wrinkled structures are generated on the surface of the silicon oxide elastic ceramic nanofiber membrane prepared by the present invention ( Figure 1 ), using the shape laser confocal microscopy system to characterize the three-dimensional morphology of the membrane material surface, it was found that the wrinkle structure was long and strip-shaped, and there were different degrees of wrinkle structures in the horizontal and vertical directions ( Figure 2 The microstructure of the silica elastic ceramic nanofiber membrane was characterized by scanning electron microscopy ( Figure 3 ), it was found that the fibers had obvious curvature bending, and the degree of bending of the ceramic fibers at the edge of the fold structure was much higher than that of the convex part inside the fold ( Figure 4 ), the fiber morphology inside the folds is similar to the conventional ceramic fiber configuration. The elastic mechanical properties of the prepared silicon oxide elastic ceramic nanofiber membrane were characterized ( Figure 5 ), under the condition of tensile strain of 40%, after cyclic stretching for 100 times, the elastic properties of the ceramic nanofiber membrane decreased slightly. After cyclic loading and unloading for 500 times, its tensile strength reached 0.92MPa, and the plastic deformation tended to be stable, which was only about 7.5%, indicating that the prepared elastic ceramic nanofiber membrane has very excellent elastic recovery properties. Example 3
[0023] S1, dissolving shape memory polymer polystyrene in a solvent of N,N-dimethylformamide and tetrahydrofuran (the mass ratio of shape memory polymer to solvent is 1:6), stirring at 400 r / min for 6 hours at room temperature to obtain a polymer sacrificial template spinning solution A; S2, adding 15g of zirconium acetate into a neutral hydrolysis system (the mass fraction of water in the ceramic precursor solution is 2%) to prepare a zirconium oxide ceramic precursor solution, which is then mixed with a polyethylene oxide aqueous solution of a spinning aid polymer (the mass ratio of the polymer to the solvent is 1:1.5), and stirred at 300r / min at room temperature for 1h to obtain a polymer / ceramic precursor (mass ratio of 30:1) solution B; S3. Electrospinning of solution A and solution B in the form of a polymer / ceramic-polymer / ceramic nanofiber sandwich membrane was performed under the conditions of a humidity of 30±10% and a temperature of 25±2°C, with silicone oil paper as the receiving substrate, the injection speed was set to 2mL / h, the receiving distance was set to 25cm, the receiving speed was 100r / min, the spinning voltage of the first layer solution A was +20kV / -1.3kV, the spinning voltage of the second layer solution A and solution B was +25kV / -3.0kV, the spinning voltage of the third layer solution B was +25kV / -3.0kV, the spinning time of each layer was 30min, and then it was peeled off from the silicone oil paper and placed in an oven at 60°C for 6h to obtain a polystyrene / zirconia-polystyrene / zirconia nanofiber sandwich membrane C; S4. Place the polystyrene / zirconia-polystyrene / zirconia nanofiber sandwich membrane C in a tubular furnace, then heat it to 800°C at a heating rate of 10°C / min under a nitrogen atmosphere, keep it warm for 3 hours, then switch to an air atmosphere, keep it warm for another 3 hours, then cool it down naturally to obtain a zirconia elastic ceramic nanofiber membrane. Example 4
[0024] S1, dissolving shape memory polymer polystyrene in a solvent of N,N-dimethylformamide and tetrahydrofuran (the mass ratio of shape memory polymer to solvent is 1:3), stirring at 400 r / min for 6 hours at room temperature to obtain a polymer sacrificial template spinning solution A; S2, adding 4.3g of tetraethoxysilane into an acidic hydrolysis system (the mass fraction of concentrated hydrochloric acid in the ceramic precursor solution is 0.3%) to prepare a silicon oxide ceramic precursor solution, which is then mixed with an aqueous solution of a spinning-aiding polymer polyvinyl alcohol (the mass ratio of the polymer to the solvent is 1:9), and stirred at 200r / min at room temperature for 1h to obtain a polymer / ceramic precursor (mass ratio of 7:3) solution B; S3. Electrospinning of solution A and solution B in the form of a polymer / ceramic-polymer / ceramic nanofiber sandwich membrane was performed under the conditions of a humidity of 30±10% and a temperature of 25±2°C, with silicone oil paper as the receiving substrate, the injection speed was set to 1 mL / h, the receiving speed was 50 r / min, the spinning voltage of the first layer solution A was +10 kV / -0.5 kV, and the receiving distance was set to 10 cm, the spinning voltage of the second layer solution A and solution B was +20 kV / -1.3 kV, and the receiving distance was set to 20 cm, the spinning voltage of the third layer solution B was +20 kV / -1.3 kV, and the receiving distance was set to 20 cm, the spinning time of each layer was 30 min, and then it was peeled off from the silicone oil paper and placed in an oven at 40°C for drying for 24 h to obtain a polystyrene / silicon oxide-polystyrene / silicon oxide nanofiber sandwich membrane C; S4. Place the polystyrene / silicon oxide-polystyrene / silicon oxide nanofiber sandwich membrane C in a tubular furnace, then heat it to 800°C at a heating rate of 5°C / min in a nitrogen atmosphere, keep it warm for 3 hours, then switch to an air atmosphere, keep it warm for another 3 hours, then cool it down naturally to obtain a silicon oxide elastic ceramic nanofiber membrane. Example 5
[0025] S1, dissolving shape memory polymer polystyrene in a solvent of N,N-dimethylformamide and tetrahydrofuran (the mass ratio of shape memory polymer to solvent is 1:13), stirring at 400 r / min for 6 hours at room temperature to obtain a polymer sacrificial template spinning solution A; S2, adding 4.3g of tetraethoxysilane into an acidic hydrolysis system (the mass fraction of concentrated hydrochloric acid in the ceramic precursor solution is 0.3%) to prepare a silicon oxide ceramic precursor solution, which is then mixed with an aqueous solution of a spinning-aiding polymer polyvinyl alcohol (the mass ratio of the polymer to the solvent is 1:9), and stirred at 200r / min at room temperature for 1h to obtain a polymer / ceramic precursor (mass ratio of 7:3) solution B; S3. Electrospinning of solution A and solution B in the form of a polymer / ceramic / polymer nanofiber sandwich membrane was performed under the conditions of a humidity of 60±10% and a temperature of 25±2°C. Silicone oil paper was used as a receiving substrate. The injection speed was set to 1 mL / h, the receiving distance was set to 20 cm, the receiving speed was 60 r / min, the spinning voltage of the first layer solution A was +15 kV / -2.0 kV, the spinning voltage of the second layer solution A and solution B was +20 kV / -1.3 kV, the spinning voltage of the third layer solution A was +15 kV / -2.0 kV, the spinning time of each layer was 30 min, and then it was peeled off from the silicone oil paper and placed in an oven at 60°C for 12 h to obtain a polystyrene / silicon oxide / polystyrene nanofiber sandwich membrane C; S4. Place the polystyrene / silicon oxide / polystyrene nanofiber sandwich membrane C in a tubular furnace, then heat it to 500°C at a heating rate of 0.5°C / min in a nitrogen atmosphere, keep it warm for 0.5h, then switch to air atmosphere, continue to keep it warm for 8h, then cool it naturally to obtain a silicon oxide elastic ceramic nanofiber membrane. Example 6
[0026] S1, dissolving shape memory polymer polystyrene in a solvent of N,N-dimethylformamide and tetrahydrofuran (the mass ratio of shape memory polymer to solvent is 1:6), stirring at 400 r / min for 6 hours at room temperature to obtain a polymer sacrificial template spinning solution A; S2, 3g of aluminum isopropoxide, 1.5g of aluminum chloride hexahydrate, and 1.5g of tetraethoxysilane were added to an acidic hydrolysis system (the mass fraction of acetic acid in the ceramic precursor solution was 0.1%) to prepare a silicon oxide ceramic precursor solution, which was then mixed with an aqueous solution of a spinning-aiding polymer polyvinyl alcohol (the mass ratio of the polymer to the solvent was 1:9), and stirred at 200r / min at room temperature for 1h to obtain a polymer / ceramic precursor (mass ratio of 6:4) solution B; S3, spray spinning of solution A and solution B in the form of a polymer / ceramic-polymer / ceramic nanofiber sandwich membrane, under the conditions of humidity of 30±10%, temperature of 25±2°C, with a breathable cage as a receiving substrate, the injection speed is set to 5mL / h, the spray pressure is 50kPa, the spray distance is 50cm, the spinning time of each layer is 30min, then it is peeled off from the breathable cage and placed in an oven at 60°C for 12h to obtain a polystyrene / mullite nanofiber sandwich membrane C; S4. Place the polystyrene / mullite-polystyrene / mullite nanofiber sandwich membrane C in a tubular furnace, then heat it to 1000°C at a heating rate of 5°C / min under a nitrogen atmosphere, keep it warm for 3 hours and then cool it naturally to obtain a mullite elastic ceramic-carbon composite nanofiber membrane. Example 7
[0027] S1, dissolving shape memory polymer polystyrene in a solvent of N,N-dimethylformamide and tetrahydrofuran (the mass ratio of shape memory polymer to solvent is 1:6), stirring at 400 r / min for 6 hours at room temperature to obtain a polymer sacrificial template spinning solution A; S2, 1.5g isopropyl titanate, 0.03g yttrium nitrate hexahydrate, and 1.7g tetraethoxysilane are added to an acidic hydrolysis system (the mass fraction of acetic acid in the ceramic precursor solution is 17%) to prepare a titanium oxide-silicon oxide ceramic precursor solution, which is then mixed with an aqueous solution of a spinning-aiding polymer polyvinyl pyrrolidone (the mass ratio of the polymer to the solvent is 1:8), and stirred at 200r / min at room temperature for 1h to obtain a polymer / ceramic precursor (mass ratio of 3:1) solution B; S3. Electrospinning of solution A and solution B in the form of a polymer / ceramic-polymer / ceramic nanofiber sandwich membrane was performed under the conditions of a humidity of 10±10% and a temperature of 20±2°C. Silicone oil paper was used as a receiving substrate. The injection speed was set to 1 mL / h, the receiving distance was set to 15 cm, the receiving speed was 60 r / min, the spinning voltage of the first layer solution A was +17 kV / -3.0 kV, the spinning voltage of the second layer solution A and solution B was +17 kV / -1.3 kV, the spinning voltage of the third layer solution A was +17 kV / -1.3 kV, the spinning time of each layer was 30 min, and then it was peeled off from the silicone oil paper and placed in an oven at 60°C for 12 h to obtain a polystyrene / titanium oxide-silicon oxide-polystyrene / titanium oxide-silicon oxide nanofiber sandwich membrane C; S4. Place the polystyrene / titanium oxide-silicon oxide-polystyrene / titanium oxide-silicon oxide nanofiber sandwich membrane C in a tubular furnace, then heat it to 600°C at a heating rate of 5°C / min under a nitrogen atmosphere, keep it warm for 3 hours and then cool it naturally to obtain a titanium oxide-silicon oxide composite elastic ceramic-carbon nanofiber membrane.
Claims
1. A method for preparing an elastic ceramic nanofiber membrane material, characterized in that: The following steps are involved: S1, dissolving a high molecular weight heat shrinkable shape memory polymer in a solvent, and stirring evenly to obtain a polymer sacrificial template spinning solution A; S2, adding the ceramic source component into a certain hydrolysis system to prepare a precursor solution containing the ceramic source component, and then mixing the precursor solution with a spinning aid polymer solution, and stirring evenly to obtain a polymer / ceramic precursor solution B; S3, performing multi-layer combined spinning on solution A and solution B, peeling them off from the receiving substrate after a certain period of time, and then placing them in an oven at a certain temperature for a period of time to dry, thereby obtaining a multilayer ceramic precursor nanofiber membrane C; S4. calcining the obtained multilayer ceramic precursor nanofiber membrane C under a certain atmosphere for a period of time to prepare an elastic ceramic nanofiber membrane material.
2. The method for preparing the elastic ceramic nanofiber membrane material according to claim 1, characterized in that: In the S1, the polymer heat-shrinkable shape-memory polymer is at least one of polyurethane, polymethoxysilane, polyethylene, polystyrene, polyvinyl chloride, polypropylene, acrylonitrile-butadiene-styrene copolymer, styrene-butadiene-styrene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polydimethyl terephthalate, polybutylene terephthalate, polylactic acid, polyvinyl pyrrolidone, polycaprolactone, and polyoxymethylene; the solvent is at least one of water, anhydrous ethanol, isopropanol, acetone, N,N-dimethylformamide, dichloromethane, tetrahydrofuran, toluene, and acetylacetone, and the mass ratio of the polymer heat-shrinkable shape-memory polymer to the solvent is 1:3 to 1:
13.
3. The method for preparing the elastic ceramic nanofiber membrane material according to claim 1, characterized in that: In the S2, the high molecular polymer is at least one of polyvinyl alcohol, polyvinyl butyral, polyvinyl pyrrolidone, polyethylene oxide, polyethylene glycol, and polyvinyl acetate; the solvent is at least one of water, anhydrous ethanol, isopropanol, acetone, N,N-dimethylformamide, dichloromethane, tetrahydrofuran, toluene, and acetylacetone, and the mass ratio of the high molecular polymer to the solvent is 1:1.5 to 1:
9.
4. The method for preparing the elastic ceramic nanofiber membrane material according to claim 1, characterized in that: In the S2, the ceramic source components are: the silicon source is tetramethoxysilane, tetraethoxysilane, tetraethyl orthosilicate, isopropyl orthosilicate; the zirconium source is zirconium acetate, zirconium chloride; the zinc source is zinc acetate, zinc nitrate; the tin source is tin acetate, tin chloride; the aluminum source is aluminum isopropoxide, aluminum sec-butoxide, aluminum chloride, aluminum nitrate, aluminum acetate; the titanium source is titanium trichloride, titanium tetrachloride, titanium oxysulfate, titanium acetylacetonate, isopropyl titanate, tetrabutyl titanate, tetraethyl titanate, diisopropoxy diacetylacetonate titanium; the barium source is barium carbonate, Barium acetate, barium sulfate, barium nitrate, barium chloride, barium hydroxide, barium oxide; lanthanum sources are lanthanum nitrate, lanthanum sulfate, lanthanum carbonate; lithium sources are lanthanum chloride, lithium nitrate, lithium sulfate, lithium chloride; silicon carbide source is polycarbosilane; the hydrolysis system is an acidic system or a neutral system, wherein the acidic substance corresponding to the acidic system is at least one of formic acid, acetic acid, oxalic acid, concentrated phosphoric acid, and concentrated hydrochloric acid, and the substance corresponding to the neutral system is water; the mass fraction of the hydrolysis system in the precursor solution containing the ceramic source components is 0.1% to 17%.
5. The method for preparing the elastic ceramic nanofiber membrane material according to claim 1, characterized in that: In the S3, the spinning technology includes at least one of electrospinning, blow spinning and centrifugal spinning, wherein the process parameters of the electrospinning process are: ambient temperature 20-35°C, humidity 10%-60%, injection speed 0.5-2mL / h, positive voltage 10-25kV, negative voltage 0.5-3.0kV, receiving distance 12-25cm, receiving speed 50-100r / min; the process parameters of the blow spinning process are: ambient temperature 20-35°C, humidity 10%-60%, injection speed 0.5-2mL / h, positive voltage 10-25kV, negative voltage 0.5-3.0kV, receiving distance 12-25cm, receiving speed 50-100r / min; the process parameters of the blow spinning process are: ambient temperature 20-35°C, humidity 10%- 60%, injection speed 1-15mL / h, blowing pressure 20-200kPa, blowing distance 5-80cm; the process parameters of the centrifugal spinning process are: ambient temperature 20-35°C, humidity 10%-60%, feed speed 0.1-20mL / h, spinning distance 5-30cm, spinneret speed 1000-20000rpm; the receiving substrate includes at least one of silicone oil paper, release paper, non-woven fabric, tin foil, metal copper mesh, breathable cage and porous mesh curtain.
6. The method for preparing the elastic ceramic nanofiber membrane material according to claim 1, characterized in that: In the S3, the multi-layer combined spinning is one of the following structures: polymer / ceramic nanofiber double-layer membrane, polymer / ceramic-polymer / ceramic nanofiber sandwich membrane, polymer / ceramic / polymer nanofiber sandwich membrane, polymer / ceramic-polymer / polymer nanofiber sandwich membrane, ceramic / ceramic-polymer / polymer nanofiber sandwich membrane and ceramic / polymer / ceramic nanofiber sandwich membrane combination structure; the drying temperature is 40-70°C and the drying time is 6-24h.
7. The method for preparing the elastic ceramic nanofiber membrane material according to claim 1, characterized in that: In the S4, the calcination atmosphere is an inert atmosphere or an inert atmosphere converted to an oxidizing atmosphere, wherein the inert atmosphere is at least one of nitrogen and argon, and an elastic ceramic-carbon composite nanofiber membrane is obtained after calcination under an inert atmosphere; the oxidizing atmosphere is at least one of air and oxygen, and a pure inorganic elastic ceramic nanofiber membrane is obtained after calcination under an oxidizing atmosphere; the calcination temperature is gradually increased from room temperature to 500-1000°C, the heating rate is 0.5-10°C / min, and the insulation time is 0.5-8h.
Citation Information
Patent Citations
Method for manfacturing ceramic-based composite material
CN107074668A
Multilayer polymer nanocomposite and preparation method thereof
CN110341205A
High-dielectric elastic composite material as well as preparation method and application thereof
CN112918031A
Super-elastic flexible three-dimensional composite ceramic nanofiber block as well as preparation method and application thereof
CN113149615A
Elastic ceramic nanofiber membrane formed by crimped fibers and preparation method and application thereof
CN118109967A
Cited By
High-elasticity RAG: W elastic ceramic, preparation method and application
CN119899033A
Preparation equipment and manufacturing method of curved-surface high-temperature-resistant polymer precursor ceramic thin film sensor
CN120400834A