Washable photochromic fiber and preparation method thereof

By coating the fiber surface with PDMS to form a hydrophobic layer and adding CuCl, the problem of slow bleaching of inorganic photochromic materials is solved, enabling rapid coloring and multiple uses of washable photochromic fibers, and improving their performance in wearable and smart display applications.

CN118957976AActive Publication Date: 2024-11-15WUHAN TEXTILE UNIV

Patent Information

Application Number
CN202411135022.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-15
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

Existing organic photochromic materials are toxic, have poor light fatigue resistance, are expensive, and have complex synthesis routes, while inorganic photochromic WO3 faces challenges in rapid bleaching, and traditional photochromic fibers are difficult to wash and reuse.

Method used

Using fiber as the substrate, a photochromic solution was synthesized at room temperature. An appropriate amount of CuCl was added to form CuCl4- complex ions to accelerate bleaching. PDMS was then coated on the fiber surface to form a hydrophobic layer, thus preparing a washable photochromic fiber.

Benefits of technology

It enables rapid coloring and bleaching of photochromic fibers, maintaining color stability of over 95%, and allows for multiple washes and reuses, making it suitable for wearable and smart display materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957976A_ABST
    Figure CN118957976A_ABST
Patent Text Reader

Abstract

The invention provides a washable photochromic fiber and a preparation method thereof. The preparation method comprises the following steps: synthesizing a tungstic acid solution at room temperature, and obtaining a WO3 solution at room temperature; the preparation method comprises the following steps: soaking fibers in a prepared solution, taking out the fibers, naturally air-drying the fibers to obtain photochromic fibers, and coating the fibers with polydimethylsiloxane with a certain concentration, so that the fibers have certain hydrophobicity and washing stability. The preparation method provided by the invention is simple to operate, non-toxic and harmless, and can be used for large-scale preparation, and the prepared photochromic fiber has good flexibility and stable photochromic performance. By adding a proper amount of CuCl, rapid coloring and bleaching are realized, and the color bleaching efficiency is greatly improved; and by using the polydimethylsiloxane for coating, the washing recycling is realized. The prepared photochromic fiber has weaving property and direct wearable property, and can be used for future intelligent clothing and implantable display application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photochromic fibers, and in particular to a washable photochromic fiber and a preparation method thereof. Background Art

[0002] Photochromism refers to the fact that under the irradiation of light of a certain wavelength and intensity, certain materials will undergo molecular structural changes or electronic changes, causing these materials to show different color changes. After years of development, although photochromic materials have gradually increased, the disadvantages of organic materials are mainly concentrated in certain toxicity, poor light fatigue resistance, high prices, and complex synthesis routes. In comparison, the performance of inorganic materials will be significantly improved.

[0003] WO3 has been widely studied for its excellent performance in electrochromism and photochromism. The crystallinity and size of WO3 have a significant impact on its photochromic properties. Photochromic WO3 has the characteristics of crystalline structure and large size, which can be triggered by ultraviolet light to achieve color change, but how to quickly bleach it is a major challenge. Summary of the invention

[0004] In view of the defects of the above-mentioned prior art, the purpose of the present invention is to provide a washable photochromic fiber and a preparation method thereof. The preparation method uses fiber as a substrate, synthesizes a photochromic solution at room temperature, and greatly improves the color bleaching efficiency by adding an appropriate amount of CuCl; and a layer of PDMS is coated on the surface of the fiber to make the fiber hydrophobic, thereby achieving the water washing and reuse of the photochromic fiber, and the color stability can be maintained at more than 95%. The washable photochromic fiber prepared by the present invention can be sewn on clothing as an ultraviolet display material, which greatly improves its application in the direction of wearable and smart display.

[0005] To achieve the above object, the present invention provides a method for preparing a washable photochromic fiber, comprising the following steps:

[0006] S1, performing surface decontamination treatment on the fiber;

[0007] S2, preparing a sodium tungstate dihydrate solution of a predetermined concentration and adding oxalic acid, and stirring evenly to obtain a mixed solution;

[0008] S3, adding hydrochloric acid to the mixed solution obtained in step S2 to adjust the pH value to 1.0-1.3;

[0009] S4, adding nickel nitrate hexahydrate to the solution obtained in step S3, and stirring to react;

[0010] S5, adding cuprous chloride to the solution obtained in step S4, and stirring to react;

[0011] S6, soaking the fiber after the decontamination treatment in step S1 in the solution obtained in step S5 for reaction, taking it out and air-drying it under natural conditions to obtain a photochromic fiber;

[0012] S7, preparing polydimethylsiloxane of a predetermined concentration and adding a curing agent; immersing the photochromic fiber obtained in step S6 in the polydimethylsiloxane solution once, taking it out and naturally air-drying it at room temperature to obtain a water-washable photochromic fiber.

[0013] As a further improvement of the present invention, in step S5, the mass fraction of the cuprous chloride is 1-4%, and the stirring reaction time is 5-10 minutes.

[0014] As a further improvement of the present invention, in step S7, the volume fraction of the PDMS is 10-20%, the solvent is n-hexane, and the amount of the added curing agent accounts for 10wt% of the PDMS.

[0015] As a further improvement of the present invention, in step S2, the concentration of the sodium tungstate dihydrate solution is 0.1-0.2 mol / L, the solvent used is deionized water; the mass fraction of the added oxalic acid relative to the added sodium tungstate dihydrate is 6.7-13.4wt%.

[0016] As a further improvement of the present invention, in step S3, the concentration of the added hydrochloric acid is 2-3 mol / L, and the stirring reaction time is 10-15 min.

[0017] As a further improvement of the present invention, in step S4, the mass fraction of the nickel nitrate hexahydrate is 10-20 wt %, and the stirring reaction time is 20-30 min.

[0018] As a further improvement of the present invention, in step S7, the curing agent is butyl fluoride silane (BFS), hydrosilane or organic peroxide.

[0019] As a further improvement of the present invention, in step S1, the surface decontamination treatment of the fiber is to place the fiber in a solution with a volume ratio of ethanol: water = 7:3 and ultrasonicate for 20 minutes to remove dust and oil on the fiber surface.

[0020] As a further improvement of the present invention, the fiber is a hydrophilic flexible fiber such as cotton fiber, polyester blended fiber, hemp fiber, bamboo fiber, etc.

[0021] To achieve the above-mentioned purpose, the present invention also provides a washable photochromic fiber, which is prepared by the preparation method described in any of the technical schemes in the aforementioned technical schemes. The washable photochromic fiber includes a fiber substrate, a color-changing layer coated on the fiber substrate, and a waterproof coating formed by polydimethylsiloxane.

[0022] The beneficial effects of the present invention are:

[0023] 1. The preparation method of washable photochromic fiber provided by the present invention can synthesize photochromic solution at room temperature, which not only saves energy but also has low cost; by adding an appropriate amount of CuCl, the recovery bleaching process of WO3 film is accelerated. The introduction of Cu ions increases the average size of nanoparticles in the film, and there are still a considerable number of small-sized nanoparticles (≈1-2nm) around the larger nanoparticles. They are quickly colored after ultraviolet light irradiation and can quickly return to colorless after the UV light source is removed. At the same time, the tetrachlorocopper complex ion [CuCl4] formed by the combination of chloride ions and divalent copper ions 2 - Make the color lighter, the color change more obvious, and significantly shorten the fading time of WO3 after color change; a certain concentration of PDMS is coated on the surface of the original photochromic fiber to make the fiber hydrophobic, so that the photochromic fiber can be washed and reused, and the color stability can be maintained at more than 95%. At the same time, the flexibility and mechanical strength of the fiber are not changed, and it can be woven and patterned at will, and can be sewn on clothing as a UV display material, which greatly improves its application in wearable and smart display directions.

[0024] 2. The present invention uses cotton fiber or the like as a substrate and obtains the photochromic fiber by an immersion method, which is not only simple to operate but also can be mass-produced.

[0025] 3. The washable photochromic fiber prepared by the present invention not only has a fast response to UV, but also has a significantly improved bleaching rate, and can be washed and recycled for multiple times, greatly improving its application performance in wearable and display applications. After irradiating the photochromic fiber with a 365nm ultraviolet lamp for 3 to 5 seconds, the fiber changes from white to light blue; after irradiation for 20 to 30 seconds, the color of the fiber deepens and becomes dark blue.

[0026] 4. The washable photochromic fiber prepared by the present invention can be quickly bleached to the original white color under natural conditions after coloring. It only takes 30 to 60 seconds for light blue to white and 3 to 5 minutes for dark blue to white. Compared with the existing WO3 photochromic material, the color bleaching efficiency is greatly improved.

[0027] 5. After the washable photochromic fiber prepared by the present invention is washed 10 times, the fiber is colored and faded again, and its stability remains almost unchanged, indicating that the PDMS layer on its surface improves its hydrophobicity and makes it washable and stable. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the SEM image of the photochromic fiber prepared in Example 1.

[0029] Figure 2 This is a physical picture of the color change and water washing performance of the photochromic fiber prepared in Example 1.

[0030] Figure 3 This is a real-life color change display of the sample of Example 1.

[0031] Figure 4 1 is the stress-strain curve of different photochromic fibers prepared in Example 1.

[0032] Figure 5 This is the SEM image of the photochromic fiber prepared in Comparative Example 1 without adding Ni(NO3)2·6H2O.

[0033] Figure 6 This is a graph showing the color changing ability of the photochromic fiber prepared in Comparative Example 2 without adding CuCl.

[0034] Figure 7 This is a photochromic fiber prepared without PDMS in Comparative Example 4, showing the actual color change before and after 10 washes.

[0035] Figure 8 This is the SEM image of the photochromic fiber prepared in Example 2.

[0036] Fig. 9 This is the SEM image of the photochromic fiber prepared in Example 3.

[0037] Fig.10 This is the SEM image of the photochromic fiber prepared in Example 4.

[0038] Fig.11 This is the SEM image of the photochromic fiber prepared in Example 5.

[0039] Fig.12 This is a physical picture of the coloring performance of the photochromic fiber prepared in Comparative Example 5 before and after washing 10 times. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0041] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0042] The present invention provides a method for preparing washable photochromic fibers, comprising the following steps:

[0043] S1, performing surface decontamination treatment on the fiber;

[0044] The fiber was placed in a solution with a volume ratio of ethanol: water = 7:3 and ultrasonicated for 20 minutes to remove dust, oil, etc. on the fiber surface.

[0045] The fibers are cotton fibers, polyester blended fibers, linen fibers, bamboo fibers and other hydrophilic flexible fibers.

[0046] S2, preparing a sodium tungstate dihydrate solution of a predetermined concentration and adding oxalic acid, and stirring evenly to obtain a mixed solution;

[0047] Specifically, a sodium tungstate dihydrate solution with a concentration of 0.1-0.2 mol / L is prepared, the solvent used is deionized water, and stirring is performed for 5-10 minutes; the mass fraction of oxalic acid added relative to the added sodium tungstate dihydrate is 6.7-13.4wt%, and stirring is continued for 5-10 minutes.

[0048] S3, adding hydrochloric acid to the mixed solution obtained in step S2 to adjust the pH value to 1.0-1.3;

[0049] Specifically, the concentration of the added hydrochloric acid is 2-3 mol / L, and the stirring reaction time is 10-15 min.

[0050] S4, adding nickel nitrate hexahydrate to the solution obtained in step S3, and stirring to react;

[0051] Specifically, the mass fraction of nickel nitrate hexahydrate added is 10-20wt%, and the stirring reaction time is 20-30min.

[0052] S5, adding cuprous chloride to the solution obtained in step S4, and stirring to react;

[0053] Specifically, the mass fraction of cuprous chloride is 1-4wt%, and the stirring reaction time is 5-10min.

[0054] The addition of cuprous chloride accelerates the recovery bleaching process of WO3 film. The introduction of Cu ions increases the average size of nanoparticles in the film. There are still a considerable number of small-sized nanoparticles (≈1-2nm) around the larger nanoparticles. They are quickly colored after UV light exposure and can quickly return to colorless after the UV light source is removed. At the same time, the tetrachlorocopper complex ion [CuCl4] formed by the combination of chloride ions and divalent copper ions 2 -(Light yellow) makes the color lighter, the color change more obvious, and the fading time of WO3 after color change is significantly shortened.

[0055] S6, soaking the fiber after the decontamination treatment in step S1 in the solution obtained in step S5 for reaction, taking it out and air-drying it under natural conditions to obtain photochromic fiber; the soaking time is 1 to 2 minutes.

[0056] S7, preparing polydimethylsiloxane of a predetermined concentration and adding a curing agent; immersing the photochromic fiber obtained in step S6 in the polydimethylsiloxane solution once, taking it out and naturally air-drying it at room temperature to obtain a water-washable photochromic fiber.

[0057] Specifically, the volume fraction of PDMS is 10-20%, the solvent is n-hexane, and the amount of the added curing agent accounts for 10wt% of the PDMS.

[0058] The curing agent is butyl fluoride silane (BFS), hydrosilane or peroxide (such as organic peroxide) and the like.

[0059] The washable photochromic fiber prepared according to the above method comprises a fiber substrate, a color-changing layer coated on the fiber substrate, and a waterproof coating formed by polydimethylsiloxane.

[0060] The preparation method of the washable photochromic fiber provided by the present invention is described below with reference to specific embodiments.

[0061] Example 1

[0062] This embodiment provides a method for preparing a washable photochromic fiber, comprising the following steps:

[0063] S1, take 10cm cotton fiber and place it in a solution with a volume ratio of ethanol: water = 7:3 and ultrasonicate for 20 minutes to remove dust and oil on the fiber surface;

[0064] S2, prepare a sodium tungstate dihydrate solution with a concentration of 0.18 mol / L with deionized water, stir for 5 minutes; and add 6.7 wt% oxalic acid dihydrate, and stir for another 5 minutes;

[0065] S3, adding 3 mol / L hydrochloric acid to the solution obtained in step S2, adjusting the pH of the solution to 1.2±0.05, and continuing stirring for 10 min to obtain a light yellow transparent solution;

[0066] S4, adding 20 wt % nickel nitrate hexahydrate to the solution obtained in step S3, stirring for 20 min, to obtain a green transparent solution;

[0067] S5, adding 3 wt % cuprous chloride to the solution obtained in step S4, stirring for 5 min, to obtain a dark blue solution;

[0068] S6, taking the fiber after the decontamination treatment in step S1 and soaking it in the dark blue solution obtained in step S5 for 1 minute, taking it out and drying it naturally at room temperature to obtain a white fiber with photochromic response.

[0069] S7, prepare a PDMS solution with a volume fraction of 10% with n-hexane, add a curing agent (PDMS: curing agent = 10:1), soak the fiber obtained in step S6 in the PDMS solution once and then take it out, and air dry it at 25°C to obtain a washable photochromic fiber. The curing agent is butyl fluoride silane (BFS).

[0070] See also Figure 1 , which is a SEM image of the photochromic fiber after adding 20 wt % Ni(NO 3 ) 2 · 6H 2 O and 3 wt % CuCl in Example 1 and using 10 wt % PDMS as a sealing layer.

[0071] It can be seen from the figure that the surface of the cotton fiber is evenly covered with a photochromic layer with a certain thickness. It can be seen that obvious WO3 particles are attached to the fiber photochromic coating and are evenly distributed. In addition, the PDMS film of this concentration has little effect on the thickness of the fiber surface film, maintaining the good flexibility of the cotton fiber.

[0072] See also Figure 2 As shown in the figure, the photochromic fiber prepared in Example 1 shows its discoloration and washing performance. It can be seen from the figure that the cotton fiber prepared in Example 1 is still white in its initial color; after being irradiated with a 365nm ultraviolet lamp for 30 seconds, it reaches the maximum color state, and it can be seen that the fiber turns obviously blue-black; after being placed under natural conditions for 3 minutes, it completely fades and the fiber returns to white. This is due to the addition of a small amount of Cu + The ions accelerate the reduction and natural oxidation process of WO3.

[0073] After washing the fiber 10 times, the fiber was colored and faded again, and its stability remained almost unchanged, indicating that the PDMS layer on its surface improved its hydrophobicity and made it water-washable and stable.

[0074] See also Figure 3 As shown, it is a real color change display diagram of the sample of Example 1. It can be seen that the pattern sewn with the color-changing fiber can change from white to obvious dark blue after being irradiated with ultraviolet light for about 20 seconds, and has good flexibility and weavability, and has good application prospects in pattern design.

[0075] See also Figure 4 As shown, it is the stress-strain curve of different photochromic fibers in Example 1. The tensile strength of the original cotton thread is 210Mpa, and its tensile strength becomes 195Mpa after absorbing the color-changing solution. After the surface is coated with 10% PDMS film, its tensile strength is significantly increased to 380Mpa, and its elongation at break is also significantly increased.

[0076] This indicates that the photochromic fiber prepared in Example 1 improves the mechanical properties of the original fiber.

[0077] Comparative Example 1

[0078] Comparative Example 1 provides a method for preparing washable photochromic fibers. Compared with Example 1, the difference is that in step S4, Ni(NO3)2·6H2O is not added. The rest is substantially the same as Example 1 and will not be described again.

[0079] See also Figure 5 The figure shows the SEM image of the photochromic fiber prepared without adding Ni(NO3)2·6H2O in Comparative Example 1. Without adding Ni, the film thickness on the fiber surface is small, and no obvious WO3 particles are seen. The flakes may be due to the uneven coating of PDMS. However, due to the small number of effective particles on its surface, the coloring time is also significantly increased, and it takes 5 minutes to color to dark blue.

[0080] Comparative Example 2

[0081] Comparative Example 2 provides a method for preparing a washable photochromic fiber. Compared with Example 1, the difference is that in step S5, CuCl is not added. The rest is substantially the same as Example 1 and will not be described again.

[0082] See also Figure 6 As shown in FIG. 2 , the color change ability of the photochromic fiber prepared without adding CuCl in comparative example 2 is displayed. Compared with example 1, after not adding CuCl, the photochromic fiber changes from white to blue-black after 60 seconds of ultraviolet light irradiation, but the bleaching time is significantly increased. Under natural conditions, its color fades to light blue after 10 minutes, and it takes more than 20 minutes to completely fade. It shows that adding a certain concentration of CuCl can greatly improve the switching efficiency of the fiber from coloring to fading.

[0083] Comparative Example 3

[0084] Comparative Example 3 provides a method for preparing a washable photochromic fiber. Compared with Example 1, the difference is that in steps S4 and S5, Ni(NO3)2·6H2O and CuCl are not added. The rest is roughly the same as Example 1 and will not be repeated here.

[0085] Experiments show that when the system does not contain Ni 2+ and Cu + When using pure WO3 film for coloring and fading, the effect is poor. The coloring time of this sample is 3-5 minutes, and the natural fading time is about 30 minutes.

[0086] Comparative Example 4

[0087] Comparative Example 4 provides a method for preparing a washable photochromic fiber. Compared with Example 1, the difference is that in step S7, PDMS is not used to encapsulate the photochromic fiber. The rest is substantially the same as Example 1 and will not be described again.

[0088] See also Figure 7 As shown, it is the actual picture of the color change of the photochromic fiber prepared without adding PDMS in Comparative Example 4 before and after washing 10 times.

[0089] It can be seen that before washing, the fiber color also changes from white to dark blue; after washing 10 times, not only the fiber surface becomes rough but also its maximum coloring state can only reach blue-gray. Compared with Example 1, its color change stability is poor. Therefore, if it is to be washable, the PDMS coated on its surface is very important.

[0090] Examples 2-5 and Comparative Example 5

[0091] The preparation method of the washable photochromic fiber provided in Examples 2-5 and Comparative Example 5 is different from that in Example 1 in that the mass fraction of Ni(NO3)2·6H2O in step S4, the mass fraction of CuCl in step S5, and the volume fraction of PDMS in step S7 are changed, as shown in the following table; the rest is roughly the same as in Example 1 and will not be repeated here.

[0092]

[0093] See also Figure 8 Shown is the SEM image of the photochromic fiber prepared in Example 2.

[0094] It can be seen that when the content of Ni(NO3)2·6H2O is reduced to 10%, the fiber surface shows larger aggregates and the WO3 layer on its surface becomes significantly thicker. Although the photochromic fiber can still achieve photochromism, its coloring time will increase by 5-10s compared with Example 1, but the coloring and fading capabilities are still good. This may be due to the fact that Ni 2+ The doping amount affects the crystal structure of WO3, thus changing the morphology of WO3.

[0095] When the content of added Ni(NO3)2·6H2O is further reduced to 8%, the stability of the precursor solution obtained in step S5 decreases, resulting in large particles gathering on the surface of the fiber immersed in the solution, affecting the bleaching rate of the discolored fiber after discoloration.

[0096] See also Fig. 9 Shown is the SEM image of the photochromic fiber prepared in Example 3.

[0097] It can be seen from the figure that WO3 particles are evenly distributed on the fiber surface, Cu + The content of Cu has little effect on the structure and morphology of WO3. The coloring and fading ability of this sample is similar to that of Example 1. + When the content is less, the bleaching and fading time will be longer than that of adding 3wt% Cu + The fading time of the sample increased by 5-10 seconds.

[0098] Example 4

[0099] This embodiment provides a method for preparing washable photochromic fibers. Compared with Embodiment 1, the difference is that in step S5, 4 wt % CuCl is added. The rest is substantially the same as Embodiment 1 and will not be described again.

[0100] See also Fig.10 The following is a SEM image of the photochromic fiber prepared in Example 4. When the CuCl content increases to 4%, the WO3 layer on the fiber surface has a rice-like particle structure. + It can accelerate the bleaching of the colored WO3 layer, but when Cu + When the concentration is too high, it will affect the darkest color of the coloring state, but the color bleaching time is shorter than that of low concentration Cu + The time can be shortened by 20-30s. Compared with Example 1, the color reaching the maximum coloring state is lighter, but the maximum absorption value of the color only differs by 0.05, which is a color change within the normal error range.

[0101] When the content of CuCl further increases to 5%, the coloring time of the color-changing fiber increases to more than 60s, and the maximum coloring state reached is much brighter than that of the low concentration CuCl. + The sample is light in color, and the color contrast before and after coloring decreases, indicating that its coloring efficiency is reduced and the color change performance is deteriorated.

[0102] Example 5

[0103] This embodiment provides a method for preparing washable photochromic fibers. Compared with Embodiment 1, the difference is that in step S7, the photochromic fibers obtained in step S6 are wrapped with a PDMS solution having a concentration of 20%. The rest is substantially the same as Embodiment 1 and will not be described again.

[0104] See also Fig.11 Shown is the SEM image of the photochromic fiber prepared in Example 5.

[0105] It can be seen from the figure that the increase in PDMS content only affects the degree of particle agglomeration on the fiber surface, but its WO3 particles are still clearly visible. The content of other particles remains unchanged and does not affect its coloring and bleaching ability.

[0106] See also Fig.12 As shown, it is a physical picture of the coloring performance of the photochromic fiber prepared in Comparative Example 5 (the photochromic fiber obtained in step S6 is wrapped with a 5% PDMS solution) before and after 10 times of water washing. It can be seen from the figure that before water washing, the photochromic fiber can change from white to blue-black under UV light, but after water washing 10 times, its maximum coloring state can only reach blue-gray. This is because the concentration of PDMS is too low, resulting in poor coating on the fiber surface, and its hydrophobic modification effect is not obvious.

[0107] In summary, the present invention provides a method for preparing washable photochromic fibers, which can synthesize photochromic solutions at room temperature, not only saving energy but also at a low cost; by adding an appropriate amount of CuCl, the switching efficiency of the fiber from coloring to fading is greatly improved, and a certain concentration of PDMS is coated on the surface of the original photochromic fiber to make the fiber hydrophobic, so that the photochromic fiber can be washed and reused, and the color stability can be maintained at more than 95%. At the same time, the flexibility and mechanical strength of the fiber are not changed, and it can be woven and patterned at will, and can be sewn on clothing as a UV display material, which greatly improves its application in wearable and smart display directions.

[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing washable photochromic fiber, characterized in that: The following steps are involved: S1, performing surface decontamination treatment on the fiber; S2, preparing a sodium tungstate dihydrate solution of a predetermined concentration and adding oxalic acid, and stirring evenly to obtain a mixed solution; S3, adding hydrochloric acid to the mixed solution obtained in step S2 to adjust the pH value to 1.0-1.3; S4, adding nickel nitrate hexahydrate to the solution obtained in step S3, and stirring to react; S5, adding cuprous chloride to the solution obtained in step S4, and stirring to react; S6, soaking the fiber after the decontamination treatment in step S1 in the solution obtained in step S5 for reaction, taking it out and air-drying it under natural conditions to obtain a photochromic fiber; S7, preparing polydimethylsiloxane of a predetermined concentration and adding a curing agent; immersing the photochromic fiber obtained in step S6 in the polydimethylsiloxane solution once, taking it out and naturally air-drying it at room temperature to obtain a water-washable photochromic fiber.

2. The method for preparing washable photochromic fiber according to claim 1, characterized in that: In step S5, the mass fraction of cuprous chloride is 1-4%, and the stirring reaction time is 5-10 minutes.

3. The method for preparing washable photochromic fiber according to claim 1, characterized in that: In step S7, the volume fraction of the polydimethylsiloxane is 10-20%, the solvent is n-hexane, and the amount of the added curing agent accounts for 10 wt % of the polydimethylsiloxane.

4. The method for preparing washable photochromic fiber according to claim 1, characterized in that: In step S2, the concentration of the sodium tungstate dihydrate solution is 0.1-0.2 mol / L, and the solvent used is deionized water; the mass fraction of the added oxalic acid relative to the added sodium tungstate dihydrate is 6.7-13.4 wt%.

5. The method for preparing washable photochromic fiber according to claim 1, characterized in that: In step S3, the concentration of the added hydrochloric acid is 2-3 mol / L, and the stirring reaction time is 10-15 min.

6. The method for preparing washable photochromic fiber according to claim 1, characterized in that: In step S4, the mass fraction of the nickel nitrate hexahydrate is 10-20 wt %, and the stirring reaction time is 20-30 min.

7. The method for preparing washable photochromic fiber according to claim 1, characterized in that: In step S7, the curing agent is butyl fluorinated silane, hydrosilane or organic peroxide.

8. The method for preparing washable photochromic fiber according to claim 1, characterized in that: In step S1, the surface decontamination treatment of the fiber is to place the fiber in a solution with a volume ratio of ethanol: water = 7:3 and ultrasonicate for 20 minutes to remove dust and oil on the fiber surface.

9. The method for preparing washable photochromic fiber according to claim 1, characterized in that: The fiber is a hydrophilic and flexible fiber.

10. A washable photochromic fiber, characterized in that: The washable photochromic fiber is prepared according to the preparation method according to any one of claims 1 to 9; the washable photochromic fiber comprises a fiber substrate, a color-changing layer coated on the fiber substrate, and a waterproof coating formed by polydimethylsiloxane.

Citation Information

Patent Citations

  • Nano WO3 photochromic powder and preparation method thereof

    CN101381599A

  • Preparation method of photochromic fiber

    CN118223287A

Cited By

  • Photochromic dispersing material, preparation method thereof and self-adaptive dimming intelligent window film prepared from photochromic dispersing material

    CN119931445A

  • A photochromic dispersion material, a preparation method thereof, and a self-adapting light-adjusting smart window film made of the same

    CN119931445B

  • Photochromic dispersion material, preparation method therefor, and self-adaptive light-modulation smart window film prepared therefrom

    WO2026184096A1