Thin film lithium niobate electro-optic phase modulator and preparation method thereof
Through the combination of thin-film lithium niobate material with diffusion and ridge optical waveguides, combined with proton exchange and dry etching technology, the problems of large size and low integration of existing lithium niobate optical phase modulator devices are solved, and a single Polarization characteristics and high integration reduce production costs and optical transmission losses.
Patent Information
- Application Number
- CN202411139136.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-15
AI Technical Summary
The existing lithium niobate optical phase modulator devices are large in size, low in integration, and the surface of the ridge optical waveguide is rough, making it difficult to accurately control the etching process, resulting in large optical transmission loss and small polarization extinction, limiting the application of single-polarization phase modulators. .
The phase modulator is prepared by thin-film lithium niobate material, combining diffusion and ridge optical waveguide structures, and through proton exchange and dry etching processes, an inverted cone optical waveguide transition structure is formed to achieve single polarization characteristics and miniaturization and high integration. , compatible with CMOS processes to achieve mass production.
The device volume is reduced to one-third, which reduces production costs, improves the overlap between the light field and the electric field and the binding ability of the optical waveguide, and realizes the single polarization transmission and efficient modulation efficiency of light.
Smart Images

Figure CN118963007A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of integrated optoelectronics, and in particular relates to a thin-film lithium niobate electro-optical phase modulator and a preparation method thereof. Background Art
[0002] The electro-optic phase modulator with single polarization characteristics is a commonly used device in optical systems. Because it can modulate the phase characteristics of light waves, it has important application value in optical communications, high-power laser synthesis, lidar, precision measurement and sensing. The phase modulator based on the electro-optic effect of lithium niobate has the advantages of large bandwidth and low insertion loss. Therefore, lithium niobate materials have been widely used in the preparation of electro-optic phase modulators. At present, most phase modulators are made of lithium niobate crystal materials, and generally adopt proton exchange or titanium diffusion optical waveguide structure. However, the refractive index difference of the lithium niobate optical waveguide formed in this way is small, and the restriction on light is weak. Therefore, the optical mode field area is large and the electro-optical overlap is low, resulting in large size and low integration of phase modulator devices based on lithium niobate crystal materials, which limits its development and application.
[0003] In recent years, the development of lithium niobate thin film materials on insulators has provided a new technical path for the miniaturization and integration of electro-optical modulation devices. Compared with lithium niobate crystal materials, thin film materials can confine the light field to micrometers or even submicrometers while retaining the inherent characteristics of lithium niobate, which can greatly improve the overlap between the light field and the electric field and achieve high-speed electro-optical conversion; in addition, due to the high refractive index difference between lithium niobate and the insulator (silicon dioxide) in the thin film material, its optical waveguide has a stronger binding ability for the light field, which can achieve the development of devices towards miniaturization and high integration. However, lithium niobate thin film materials generally use etching processes to prepare ridge optical waveguides. The surface of the optical waveguide prepared by this method is rough and there are products. It is difficult to accurately control its etching process, which increases the light transmission loss; secondly, the ridge optical waveguide formed by etching can simultaneously support the transmission of TE and TM polarized light during light transmission. The polarization extinction of the device is relatively small, which limits the application of single polarization phase modulators. Summary of the invention
[0004] The present invention aims to provide a thin-film lithium niobate electro-optic phase modulator and a preparation method thereof, which improves the modulation efficiency, has a single polarization characteristic, reduces the device size, achieves compatibility with existing semiconductor processes and enables mass production.
[0005] In order to achieve the purpose of the present invention, the present invention provides a method for preparing a thin film lithium niobate electro-optical phase modulator, comprising the following steps:
[0006] S1: providing a thin film lithium niobate wafer, cleaning and drying;
[0007] S2: preparing a thin film lithium niobate diffused optical waveguide mask 8;
[0008] S3: Preparation of thin film lithium niobate diffused optical waveguide 7;
[0009] S4: preparing a phase modulation region ridge type optical waveguide mask 8;
[0010] S5: preparing a phase modulation region ridge type optical waveguide 6;
[0011] S6: preparing a cladding layer 4 on the chip;
[0012] S7: preparing the modulation region electrode 5;
[0013] S8: Slice and cleave the prepared thin-film lithium niobate wafer, polish both ends of the diced thin-film lithium niobate wafer slices, and complete the production of the thin-film lithium niobate electro-optical phase modulator.
[0014] Further, the S2 comprises the following steps:
[0015] S2-1: growing a diffusion type optical waveguide mask on the surface of the thin film lithium niobate wafer, the thickness of which is 100-300 nm;
[0016] S2-2: preparing a diffusion type optical waveguide pattern on the diffusion type optical waveguide mask by photolithography and development;
[0017] S2-3: etching the area not covered by the photoresist by dry etching, and the etching depth must be the same as the thickness of the diffusion type optical waveguide mask;
[0018] S2-4: Removing the residual photoresist, the diffusion type optical waveguide mask 8 is completed.
[0019] Furthermore, the S3 is specifically as follows: placing the thin film lithium niobate wafer into a proton exchange furnace for proton exchange, and then annealing in a tubular annealing furnace, and the diffusion type optical waveguide is prepared.
[0020] Furthermore, the proton source 9 is a mixture of benzoic acid and lithium benzoate, the proton exchange temperature is 230-245° C., and the proton exchange time is 1-3 h; the annealing environment is an oxygen atmosphere, the annealing temperature is 300-400° C., and the annealing time is 3-5 h.
[0021] Further, the S4 comprises the following steps:
[0022] S4-1: growing a ridge-type optical waveguide mask with a thickness of 600-1000 nm on the surface of the thin-film lithium niobate wafer on which the diffused optical waveguide 7 is prepared;
[0023] S4-2: preparing a ridge type optical waveguide pattern on the ridge type optical waveguide mask by photolithography and development;
[0024] S4-3: etching the area not covered by the photoresist by dry etching, and the etching depth must be the same as the thickness of the ridge optical waveguide mask;
[0025] S4-4: Removing the residual photoresist, the ridge-type optical waveguide mask 8 is completed.
[0026] Furthermore, the S5 uses argon ion-based dry etching to etch the ridge-type optical waveguide pattern, and then removes the ridge-type optical waveguide mask, and the ridge-type optical waveguide 6 is prepared.
[0027] Furthermore, the S6 specifically comprises growing a high-quality silicon oxide upper cladding layer 4 on the surface of the thin-film lithium niobate wafer on which the diffused optical waveguide is made, and the thickness of the upper cladding layer 4 is 200-800 nm.
[0028] Further, the S7 comprises the following steps:
[0029] S7-1: sputtering a layer of WTi / Au with a thickness of 100 / 80 nm on the surface of the thin film lithium niobate wafer;
[0030] S7-2: preparing a desired pattern of a modulation electrode in a modulation area on the surface by photolithography and development;
[0031] S7-3: After the photolithography is completed, the thin-film lithium niobate wafer is placed in the electroplating solution for gold electroplating, and then the surface photoresist is removed, and then the WTi / Au is etched clean. At this time, the electrode 5 in the modulation area is completed.
[0032] On the other hand, the present invention also provides a thin-film lithium niobate electro-optic phase modulator, comprising a substrate 1, an insulating layer 2, a lithium niobate thin film 3, an upper cladding layer 4, a modulation electrode 5, a ridge optical waveguide 6, and a diffusion optical waveguide 7;
[0033] The substrate 1 is silicon or lithium niobate;
[0034] The insulating layer 2 is made of silicon dioxide and has a thickness of 2 to 5 μm;
[0035] The lithium niobate film 3 has a thickness of 5 to 10 μm and a tangent direction of X;
[0036] The upper cladding layer 4 is silicon dioxide, and its thickness is 200 to 800 nm;
[0037] The modulation electrode 5 is a push-pull electrode structure, and the electrode thickness is 10-15 μm;
[0038] The ridge type optical waveguide 6 and the diffusion type optical waveguide 7 are used as the optical waveguide structure of the modulator.
[0039] Furthermore, the diffused optical waveguide is used at the input and output ends, and the ridged optical waveguide is used in the modulation area; the diffused optical waveguide has a depth of 2 to 4 μm, and the ridged optical waveguide has a depth of 2 to 4 μm; an inverted cone optical waveguide transition structure is used between the two optical waveguide structures.
[0040] Compared with the prior art, the significant progress of the present invention is as follows: (1) the phase modulator prepared by the present invention using thin-film lithium niobate material can reduce the volume size to one third compared with the electro-optic phase modulator prepared by traditional lithium niobate bulk material; (2) the present invention adopts a scheme combining a diffuse waveguide with a ridge waveguide, which not only retains the advantages of low transmission loss and low coupling loss of the diffuse waveguide, but also takes advantage of the small width and stronger light localization ability of the ridge waveguide; (3) the electro-optic phase modulator structure provided by the present invention can realize single-polarization transmission of light; (4) the electro-optic phase modulator preparation method provided by the present invention adopts CMOS-compatible processes, which can realize wafer-level mass production and significantly reduce the production cost of the modulator.
[0041] In order to more clearly illustrate the functional characteristics and structural parameters of the present invention, further description is given below in conjunction with the accompanying drawings and specific implementation methods. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0043] Figure 1 is a side view of the thin-film lithium niobate electro-optic phase modulator of the present invention;
[0044] Figure 2 is a top view of the thin-film lithium niobate electro-optic phase modulator of the present invention;
[0045] Figure 3 (a)-(h) are flow charts of the method for preparing the thin-film lithium niobate electro-optic phase modulator of the present invention.
[0046] The reference numerals in the figure are: 1-substrate, 2-insulating layer, 3-lithium niobate film, 4-upper cladding, 5-modulation electrode, 6-ridge type optical waveguide, 7-diffusion type optical waveguide, 8-hard mask, 9-proton source. DETAILED DESCRIPTION
[0047] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0048] Combination Figure 1 and Figure 2 , as shown in the figure, a thin-film lithium niobate electro-optic phase modulator provided by this embodiment includes a substrate 1, an insulating layer 2, a lithium niobate thin film 3, an upper cladding layer 4, a modulation electrode 5, a ridge optical waveguide 6, and a diffusion optical waveguide 7;
[0049] The substrate 1 is silicon or lithium niobate; the insulating layer 2 is silicon dioxide with a thickness of 2 to 5 μm; the lithium niobate film 3 is 5 to 10 μm thick and has an X-cut direction; the upper cladding 4 is silicon dioxide with a thickness of 200 to 800 nm; the modulation electrode 5 is a push-pull electrode structure with an electrode thickness of 10 to 15 μm; the ridge-type optical waveguide 6 and the diffusion-type optical waveguide 7 are used as the optical waveguide structure of the modulator.
[0050] The diffused optical waveguide 7 is used at the input and output ends, and the ridge-type optical waveguide 6 is used in the modulation area; the depth of the diffused optical waveguide 7 is 2 to 4 μm, and the depth of the ridge-type optical waveguide 6 is 2 to 4 μm; an inverted cone optical waveguide transition structure is used between the two optical waveguide structures. Among them, the transmission light is input from the left side of the modulator chip and output from the right side of the modulator chip. The input and output ends adopt an inverted cone structure, the optical waveguide type is a diffused optical waveguide, and the optical waveguide is surrounded by a lithium niobate film layer; the modulation area adopts a straight optical waveguide structure, and the optical waveguide type is a composite structure of a diffused optical waveguide and a ridge-type optical waveguide. After the optical waveguide is subjected to the proton exchange process, it is dry-etched into a ridge-type structure.
[0051] Combination Figure 3 , a method for preparing a thin film lithium niobate electro-optic phase modulator, comprising the following steps:
[0052] S1: Figure 3 As shown in (a), a thin-film lithium niobate wafer is prepared, wherein the structure includes a silicon substrate 1, a silicon dioxide insulating layer 2 and a lithium niobate thin film 3, and the wafer is ultrasonically cleaned with acetone, ethanol and deionized water and then dried;
[0053] S2: Figure 3 As shown in (b), a dense silicon dioxide film is grown on the surface of the thin-film lithium niobate wafer, and the film thickness is 200-300nm. The pattern of the diffused optical waveguide is prepared on the silicon dioxide film by photolithography and development. Then, the area not covered by the photoresist is etched by dry etching. The etching depth needs to be the same as the thickness of the silicon dioxide film. After etching, the residual photoresist is removed. At this time, the diffused optical waveguide mask 8 is prepared;
[0054] S3: Figure 3As shown in (c), the thin film lithium niobate wafer is placed in a proton exchange furnace, the proton source 9 is a mixture of benzoic acid and lithium benzoate, the proton exchange temperature is 230-245°C, and the proton exchange time is 1-3h; the post-proton exchange annealing is completed in a tubular annealing furnace, the annealing environment is an oxygen atmosphere, the annealing temperature is 300-400°C, and the annealing time is 3-5h, at which time the diffusion type optical waveguide 7 is prepared;
[0055] S4: Figure 3 As shown in (d), a dense silicon dioxide film is grown on the surface of the thin-film lithium niobate wafer, and the film thickness is 600-1000nm. The pattern of the ridge optical waveguide is prepared on the silicon dioxide film by photolithography and development. Then, the area not covered by the photoresist is etched by dry etching. The etching depth needs to be the same as the thickness of the silicon dioxide film. After etching, the residual photoresist is removed. At this time, the ridge optical waveguide mask 8 is prepared;
[0056] S5: Figure 3 As shown in (e), the ridge-type optical waveguide is etched by using an argon ion-based dry etching process, and the photoresist used as a mask is removed after etching. At this time, the ridge-type optical waveguide 6 is completed;
[0057] S6: Figure 3 As shown in (f), a high-quality silicon oxide upper cladding layer 4 is grown on the surface of the thin-film lithium niobate wafer on which the optical waveguide is made, and the thickness of the upper cladding layer 4 is 200 to 800 nm;
[0058] S7: Figure 3 As shown in (g), a layer of WTi / Au with a thickness of 100 / 80nm is sputtered on the surface of the thin-film lithium niobate wafer, and a pattern of the modulation electrode 5 in the modulation area is prepared on the surface by a photolithography and development process. After the photolithography is completed, the thin-film lithium niobate wafer is placed in an electroplating solution for a gold electroplating process. After the electroplating, the photoresist on the surface is removed, and the WTi / Au is etched clean. At this time, the modulation electrode 5 is prepared;
[0059] S8: Figure 3 As shown in (h), the prepared thin-film lithium niobate wafer is sliced and cleaved, and the two ends of the sliced small pieces are polished and masked. At this point, a thin-film lithium niobate electro-optical phase modulator is prepared.
[0060] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0061] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a thin film lithium niobate electro-optical phase modulator, characterized in that: The following steps are involved: S1: providing a thin film lithium niobate wafer, cleaning and drying; S2: Preparation of thin film lithium niobate diffused optical waveguide mask; S3: Preparation of thin film lithium niobate diffused optical waveguide; S4: preparing a ridge-type optical waveguide mask in the phase modulation area; S5: Preparation of phase modulation region ridge optical waveguide; S6: preparing the cladding layer on the chip; S7: Preparation of modulation area electrodes; S8: Slice and cleave the prepared thin-film lithium niobate wafer, polish both ends of the diced thin-film lithium niobate wafer slices, and complete the production of the thin-film lithium niobate electro-optical phase modulator.
2. The method for preparing a thin film lithium niobate electro-optical phase modulator according to claim 1, characterized in that: The S2 comprises the following steps: S2-1: growing a diffusion-type optical waveguide mask on the surface of the thin-film lithium niobate wafer, with a thickness of 100-300 nm; S2-2: preparing a diffusion type optical waveguide pattern on the diffusion type optical waveguide mask by photolithography and development; S2-3: Etching the area uncovered by the photoresist by dry etching, wherein the etching depth must be the same as the thickness of the diffused optical waveguide mask; S2-4: Removing the residual photoresist, and the diffusion type optical waveguide mask is completed.
3. The method for preparing a thin film lithium niobate electro-optical phase modulator according to claim 1, characterized in that: The S3 specifically includes: placing the thin film lithium niobate wafer into a proton exchange furnace to perform proton exchange, and then annealing in a tubular annealing furnace, thereby completing the preparation of the diffused optical waveguide.
4. The method for preparing a thin film lithium niobate electro-optical phase modulator according to claim 3, characterized in that: The proton source is a mixture of benzoic acid and lithium benzoate, the proton exchange temperature is 230-245° C., and the proton exchange time is 1-3 hours; the annealing environment is an oxygen atmosphere, the annealing temperature is 300-400° C., and the annealing time is 3-5 hours.
5. The method for preparing a thin film lithium niobate electro-optical phase modulator according to claim 1, wherein: The S4 comprises the following steps: S4-1: growing a ridge-type optical waveguide mask with a thickness of 600-1000 nm on the surface of the thin-film lithium niobate wafer on which the diffused optical waveguide is fabricated; S4-2: preparing a ridge-type optical waveguide pattern on the ridge-type optical waveguide mask by photolithography and development; S4-3: Etching the area not covered by the photoresist by dry etching, wherein the etching depth must be the same as the thickness of the ridge optical waveguide mask; S4-4: Residual photoresist is removed, and the ridge-type optical waveguide mask is prepared.
6. The method for preparing a thin film lithium niobate electro-optical phase modulator according to claim 1, characterized in that: The S5 uses argon ion-based dry etching to etch the ridge-type optical waveguide pattern, and then removes the ridge-type optical waveguide mask, and the ridge-type optical waveguide is completed.
7. The method for preparing a thin film lithium niobate electro-optical phase modulator according to claim 1, characterized in that: The S6 specifically comprises growing a high-quality silicon oxide upper cladding layer on the surface of the thin-film lithium niobate wafer on which the diffused optical waveguide is made, wherein the thickness of the upper cladding layer is 200 to 800 nm.
8. The method for preparing a thin film lithium niobate electro-optical phase modulator according to claim 1, characterized in that: The S7 comprises the following steps: S7-1: sputtering a layer of WTi / Au with a thickness of 100 / 80 nm on the surface of the thin film lithium niobate wafer; S7-2: preparing a desired pattern of a modulation electrode in the modulation area on the surface by photolithography and development; S7-3: After the photolithography is completed, the thin film lithium niobate wafer is placed in the electroplating solution for gold electroplating, and then the surface photoresist is removed, and the WTi / Au is etched clean. At this time, the electrode preparation in the modulation area is completed.
9. A thin film lithium niobate electro-optical phase modulator, characterized in that: It comprises a substrate (1), an insulating layer (2), a lithium niobate thin film (3), an upper cladding layer (4), a modulation electrode (5), a ridge-type optical waveguide (6), and a diffusion-type optical waveguide (7); The substrate (1) is silicon or lithium niobate; The insulating layer (2) is silicon dioxide and has a thickness of 2 to 5 μm; The lithium niobate film (3) has a thickness of 5 to 10 μm and an X-cut direction; The upper cladding layer (4) is silicon dioxide, and its thickness is 200 to 800 nm; The modulation electrode (5) is a push-pull electrode structure, and the electrode thickness is 10 to 15 μm; The ridge-type optical waveguide (6) and the diffusion-type optical waveguide (7) are used as the optical waveguide structure of the modulator.
10. The thin film lithium niobate electro-optical phase modulator according to claim 9, characterized in that: The input and output ends adopt the diffusion-type optical waveguide (7), and the modulation area adopts the ridge-type optical waveguide (6); the diffusion-type optical waveguide (7) has a depth of 2 to 4 μm, and the ridge-type optical waveguide (6) has a depth of 2 to 4 μm; an inverted cone-type optical waveguide transition structure is adopted between the two optical waveguide structures.
Citation Information
Cited By
Preparation method of electro-optical modulator
CN119758620A
Silicon-based thin-film lithium niobate modulator integrated with optical storage and manufacturing method of silicon-based thin-film lithium niobate modulator
CN121879011A