Semiconductor structure and forming method thereof
By using a metal nitride layer as the outer layer structure of the side wall in a semiconductor device, the stress problem caused by the increase in the thickness of the nitride layer in the prior art is solved, and the stability and performance improvement of the semiconductor structure are achieved.
Patent Information
- Application Number
- CN202411046434.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The ONN structure of the side wall in existing semiconductor devices leads to an increase in the thickness of the nitride layer, causing greater stress, resulting in problems such as warping and deformation of wafers and degradation of performance.
The metal nitride layer is used as the outer layer structure of the side wall. The metal nitride layer is formed through the metal organic chemical vapor deposition process, and the doping process is carried out when necessary. The unnecessary layers are removed in combination with dry etching technology to form the first Side walls to reduce stress.
It effectively reduces the stress of the semiconductor structure, ensures its integrity, and improves the electrical characteristics and performance of semiconductor devices through metal nitride layers with low stress and dielectric constant.
Smart Images

Figure CN118969620A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductors, and in particular to a semiconductor structure and a method for forming the same. Background Art
[0002] In semiconductor manufacturing, a sidewall is a sidewall structure formed on the side of a structure (such as a transistor) on a substrate. The sidewall is usually composed of an insulating or conductive material layer, and its main function is to provide electrical isolation or change the electrical characteristics of the device.
[0003] However, the existing sidewall structure is an "ONN structure", that is, one oxide layer and two nitride layers, which increases the thickness of the nitride layer and brings greater stress, resulting in the risk of wafer warping and deformation or even fragmentation, affecting device performance. Summary of the invention
[0004] The technical problem solved by the present invention is to provide a semiconductor structure and a method for forming the same, so as to improve the performance of semiconductor devices.
[0005] To solve the above technical problems, an embodiment of the present invention provides a method for forming a semiconductor structure, comprising: providing a substrate, wherein the substrate includes a gate structure; forming side walls on both sides of the gate structure; forming a metal nitride layer on the surface of the substrate, the surface of the side walls, and the top surface of the gate structure; etching and removing the metal nitride layer until the surface of the substrate and the top surface of the gate structure are exposed, thereby forming a first side wall.
[0006] Optionally, the method for forming the metal nitride layer is a metal organic chemical vapor deposition process, and the parameters of the metal organic chemical vapor deposition process are: a deposition temperature of 400 degrees Celsius to 600 degrees Celsius.
[0007] Optionally, the thickness of the metal nitride layer is in a range of 400 angstroms to 500 angstroms, the stress of the metal nitride layer is in a range of 300 MPa to 600 MPa, and the dielectric constant of the metal nitride is in a range of 8 to 11.5.
[0008] Optionally, the metal nitride layer is aluminum nitride, the thickness of the aluminum nitride ranges from 400 angstroms to 500 angstroms, the stress of the aluminum nitride ranges from 300 MPa to 600 MPa, and the dielectric constant of the aluminum nitride ranges from 8.8 to 8.9.
[0009] Optionally, after the step of forming the metal nitride layer, the method further includes: performing a doping treatment on the metal nitride layer to obtain a metal doped layer.
[0010] Optionally, the process parameters of the doping treatment are: ammonia as the nitrogen source, the doping temperature is 600 degrees Celsius to 900 degrees Celsius, the pressure is 60mT to 100mT, the doping element of the doping treatment is scandium, silicon or zirconium, and the dielectric constant of the metal doping layer ranges from 8 to 11.5.
[0011] Optionally, the process of etching and removing the metal nitride layer is a dry etching process, and the process parameters of the dry etching process are that the etching gas is a combination of one or more of H2, CF4, CHF3, CH2F2, C4F8 and Ar, the gas flow rate of the etching gas is 30sccm to 80sccm, the source power is 800W to 1200W, the bias power is 100W to 400W, the etching pressure is 10mTorr to 50mTorr, and the etching time is 30 seconds to 70 seconds.
[0012] Optionally, the step of forming sidewalls on both sides of the gate structure includes: forming a silicon oxide layer on the substrate surface and the gate structure; forming a silicon nitride layer on the surface of the silicon oxide layer; and etching and removing the silicon nitride layer on the substrate until the surface of the silicon oxide layer is exposed.
[0013] Optionally, the process for forming the silicon oxide layer is high temperature furnace tube annealing, and the process parameters of the high temperature furnace tube annealing are: annealing temperature is 1015 degrees Celsius, and annealing time is 18 seconds. The process for forming the silicon nitride layer is a low pressure chemical vapor deposition process, and the parameters of the chemical vapor deposition process are: the deposition rate of the silicon nitride layer is 15.3 angstroms per minute to 16.5 angstroms per minute, and the deposition time is 392 seconds.
[0014] Optionally, the thickness of the silicon nitride layer ranges from 100 angstroms to 110 angstroms, and the thickness of the silicon oxide layer ranges from 20 angstroms to 25 angstroms.
[0015] Optionally, the process of etching and removing the silicon nitride layer is a dry etching process, and the process parameters of the dry etching process are that the etching gas is a combination of one or more of CH2F2, CHF3, O2 and He, the gas flow rate of the etching gas is 40sccm to 80sccm, the bias strategy is 50W to 150W, the source power is 600W to 850W, the etching pressure is 30mTorr to 60mTorr, and the etching time is 20 seconds to 40 seconds.
[0016] Optionally, after the step of forming the sidewalls, the method further includes: using the sidewalls as masks to perform a first ion implantation process on the substrate to form lightly doped regions located on both sides of the gate structure.
[0017] Optionally, the process parameters of the first ion implantation treatment are: implantation energy range is 4 kJ to 30 kJ, ion concentration range is 355 E3 ions / cm 2 To 460E4ions / cm 2 , the injection angle is 0 degrees to 45 degrees.
[0018] Optionally, after the step of forming the metal nitride layer, the method further includes: performing a second ion implantation process on the substrate using the first sidewall as a mask layer to form a source / drain region.
[0019] Optionally, the process parameters of the second ion implantation treatment are an implantation energy range of 6.5 kJ to 20 kJ and an ion concentration range of 200 E3 ions / cm 2 To 280E5ions / cm 2 , the injection angle is 0 degrees to 45 degrees.
[0020] Correspondingly, the present invention also provides a semiconductor structure, comprising: a substrate, wherein the substrate comprises a gate structure; a first sidewall, wherein the first sidewall comprises: sidewalls located on both sides of the gate structure, and a metal nitride layer located on the surface of the sidewall.
[0021] Optionally, the thickness of the metal nitride layer is in a range of 400 angstroms to 500 angstroms, the stress of the metal nitride layer is in a range of 300 MPa to 600 MPa, and the dielectric constant of the metal nitride is in a range of 8 to 11.5.
[0022] Optionally, the metal nitride layer is aluminum nitride, the thickness of the aluminum nitride ranges from 400 angstroms to 500 angstroms, the stress of the aluminum nitride ranges from 300 MPa to 600 MPa, and the dielectric constant of the aluminum nitride ranges from 8.8 to 8.9.
[0023] Optionally, the sidewall spacer includes: a silicon oxide layer located on the surface of the substrate and the gate structure, and a silicon nitride layer located on the surface of the silicon oxide layer.
[0024] Optionally, the first sidewall spacer includes: a silicon oxide layer located on the surfaces of the substrate and the gate structure, a silicon nitride layer located on the surface of the silicon oxide layer, and a metal nitride layer located on the surface of the silicon nitride layer.
[0025] Compared with the prior art, the technical solution of the embodiment of the present invention has the following beneficial effects:
[0026] The present invention forms a metal nitride layer on the side wall so that the outer layer structure of the first side wall formed subsequently is the metal nitride layer, thereby reducing the stress of the first side wall and ensuring the integrity of the semiconductor structure. In addition, the metal nitride layer is used as the outer layer structure of the side wall. Since the metal nitride layer has low stress and dielectric constant, the electrical characteristics of the semiconductor structure are guaranteed, thereby improving the performance of the semiconductor device.
[0027] Furthermore, the present invention introduces impurity energy levels by doping the metal nitride layer, thereby changing the charge distribution and polarization process of the metal nitride layer material, thereby adjusting the dielectric constant and improving the performance of the semiconductor device.
[0028] Furthermore, the present invention forms a silicon oxide layer on the top surface of the gate structure so that when etching the sidewalls and the metal nitride layer on the top of the gate structure, the silicon oxide layer can be used as an etching stop layer to avoid etching to the top of the gate structure, thereby ensuring the integrity of the active area. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figures 1 to 6 is a schematic diagram of a process for forming a semiconductor structure in one embodiment of the present invention. DETAILED DESCRIPTION
[0030] It should be noted that the terms “surface” and “on” in this specification are used to describe relative positional relationships in space and are not limited to direct contact.
[0031] At present, the sidewalls of the semiconductor structure are of an "ONON" structure, which are silicon oxide layer, silicon nitride layer, silicon oxide layer and silicon nitride layer, respectively. In order to reduce the thermal budget and improve device performance, the "ONON" structure is transformed into an "ONN" structure, that is, a silicon oxide layer and two silicon nitride layers. To ensure the consistency of key dimensions, the outer silicon nitride layer needs to become thicker to meet the key dimension requirements, which leads to an increase in the thickness of the silicon nitride layer. Since an excessively thick silicon nitride layer will bring greater stress, the wafer will be warped and even broken, affecting the electrical properties and reducing the reliability and stability of the product.
[0032] In order to solve the above technical problems, the technical solution of the present invention provides a semiconductor structure and a method for forming the same, wherein the metal nitride layer is used as the outer layer structure of the first side wall, so that the stress of the first side wall is reduced, thereby ensuring the integrity of the semiconductor structure. Moreover, since the metal nitride layer has low stress and dielectric constant, the electrical characteristics of the semiconductor structure are guaranteed, thereby improving the performance of the semiconductor device.
[0033] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0034] Figures 1 to 6 is a schematic diagram of a process for forming a semiconductor structure in one embodiment of the present invention.
[0035] Please refer to Figure 1 , providing a substrate 100, wherein the substrate 100 includes a P-well region 1002, an N-well region 1001, and a gate structure 102 located on the P-well region 1002 and the N-well region 1001.
[0036] In this embodiment, the substrate 100 is made of silicon.
[0037] In other embodiments, the material of the substrate 100 may also be germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium; in other embodiments, the substrate 100 may also be a silicon on insulator substrate 100 or a germanium on insulator substrate 100.
[0038] In one embodiment, it further includes: an isolation region 101 located between the adjacent P-well region 1002 and the N-well region 1001 .
[0039] The method for forming the isolation region 101 includes: etching the substrate 100 to form a shallow trench; and forming the isolation region 101 in the shallow trench.
[0040] In this embodiment, the material of the isolation region 101 is silicon oxide.
[0041] In this embodiment, the isolation region 101 is in an inverted trapezoidal shape.
[0042] The isolation region 101 is used to avoid electrical crosstalk between adjacent active devices.
[0043] In this embodiment, the method further includes: removing the isolation region 101 higher than the surface of the substrate 100 through a planarization process.
[0044] In this embodiment, the planarization process adopts a chemical mechanical polishing process.
[0045] In this embodiment, by adjusting the process parameters of chemical mechanical polishing, it is possible to ensure that during the polishing process, the isolation region 101 above the surface of the substrate 100 is removed and stops at a surface flush with the substrate 100 .
[0046] In other embodiments, the thickness of the isolation region 101 above the surface of the substrate 100 is 0 angstroms to 80 angstroms.
[0047] In this embodiment, the method for forming the P-well region 1002 and the N-well region 1001 includes: performing ion implantation on the substrate 100 to form the P-well region 1002 and the N-well region 1001 .
[0048] In this embodiment, the ion concentration range of the ion implantation treatment is 220E3ions / cm 2 To 420E3ions / cm 2 .
[0049] The method for forming the gate structure 102 includes: sequentially forming a gate oxide layer 1021 and a gate layer 1022 located on the gate oxide layer 1021 on the surface of the substrate 100 and the surface of the isolation region 101; etching the gate oxide layer 1021 and the gate layer 1022 until the substrate 100 is exposed to form the gate structure 102.
[0050] In this embodiment, the material of the gate oxide layer 1021 is silicon oxide.
[0051] In this embodiment, the material of the gate layer 1022 is polysilicon.
[0052] A dry etching process is used to etch away the gate oxide layer 1021 and the gate layer 1022 until the substrate 100 is exposed. The parameters of the dry etching process include: the chamber pressure is 5.5mT to 50mT, the source power is 180W to 1000W, the etching gas contains one or more combinations of CH2F2, Cl2, HBr, He and O2, the gas flow rate is 20sccm to 200sccm, and the etching time is 6s to 40s.
[0053] Please refer to Figure 2 , forming sidewall spacers 103 on both sides of the gate structure 102 .
[0054] The method for forming the spacer 103 includes: forming a silicon oxide layer 1031 on the P-well region 1002 , the N-well region 1001 and the gate structure 102 .
[0055] In this embodiment, the process for forming the silicon oxide layer 1031 is high temperature furnace tube annealing, and the process parameters of the high temperature furnace tube annealing are: annealing temperature is 1015 degrees Celsius, and annealing time is 18 seconds.
[0056] The thickness of the silicon oxide layer 1031 is in the range of 20 angstroms to 25 angstroms, and the density of the silicon oxide layer 1031 is 2.2 g / cm 3 Up to 2.6g / cm 3Therefore, the silicon oxide is a material with high hardness and corrosion resistance. In the subsequent process of etching the silicon nitride layer 1032, the silicon oxide layer 1031 can serve as an etching barrier to ensure that the substrate 100 is not etched. In addition, the density of the silicon oxide layer 1031 is less than the density of the silicon nitride layer 1032 to be formed subsequently, so that in the subsequent ion implantation process, the blocking ability of the silicon oxide layer 1031 to ions is less than the blocking ability of the silicon nitride layer 1032 to ions, thereby making the implantation depth under the P-well region 1002 or the N-well region 1001 below the silicon nitride layer 1032 less than the implantation depth under the P-well region 1002 or the N-well region 1001 not blocked by the silicon nitride layer 1032, thereby forming a lightly doped region and a heavily doped region (i.e., a source / drain region).
[0057] The thermal expansion coefficient of the silicon oxide layer 1031 is 0.5×10 -6 / ℃, is a material with good thermal stability and high temperature performance, so it can maintain structural stability in high temperature environment and ensure the normal operation of ion implantation.
[0058] Please refer to Figure 3 The method for forming the sidewall spacer 103 further includes: forming a silicon nitride layer 1032 on the silicon oxide layer 1031 .
[0059] In this embodiment, the process for forming the silicon nitride layer 1032 is a chemical vapor deposition process, and the parameters of the chemical vapor deposition process are: the deposition rate of the silicon nitride layer 1032 is 15.3 angstroms per minute to 16.5 angstroms per minute, and the deposition time of the silicon nitride layer 1032 is 392 seconds.
[0060] Before forming the silicon nitride layer 1032 , the method further includes: forming an initial silicon nitride layer 1032 on the silicon oxide layer 1031 ; and etching and removing the silicon nitride layer 1032 on the substrate 100 until the surface of the silicon oxide layer 1031 is exposed.
[0061] In this embodiment, the process of etching and removing the silicon nitride layer 1032 is a dry etching process, and the etching gas of the dry etching process is a mixture of one or more of CH2F2, CHF3, O2, and He. The etching gas flow rate is 40sccm to 80sccm, the bias power is 50w to 150w, the source power is 600w to 850w, the pressure is 30mTorr to 60mTorr, and the etching time is 20s to 40s.
[0062] The thickness of the silicon nitride layer 1032 is in a range of 100 angstroms to 110 angstroms.
[0063] The density range of silicon nitride is 3.24 g / cm 3Up to 3.26g / cm 3 , which makes the hardness of the silicon nitride layer 1032 greater. Since the working principle of ion implantation is to bombard semiconductor materials with high-energy ion beams, the silicon nitride layer 1032 has good mechanical strength and hardness to withstand the impact of ion beams and ensure stable operation of the equipment.
[0064] The thermal expansion coefficient of the silicon nitride layer 1032 is 2.8*10 -6 / ℃ to 3.1*10 -6 / ℃, so it has high thermal stability, enabling it to maintain structural stability in high temperature environments and ensure the normal operation of ion implantation. Secondly, the chemical stability of the silicon nitride layer 1032 ensures that it will not undergo chemical reactions during the ion implantation process, thereby avoiding adverse effects on the semiconductor film.
[0065] Please refer to Figure 4 After forming the silicon nitride layer 1032 , the method further includes: performing a first ion implantation process on the substrate 100 using the sidewall 103 as a mask to form lightly doped regions located on both sides of the gate structure 102 .
[0066] The method for forming lightly doped regions on both sides of the gate structure 102 includes: using the sidewall 103 as a mask, performing a first ion implantation process in the substrate 100 of the P-well region 1002 , and forming N-type lightly doped regions 105 in the P-well region 1002 on both sides of the sidewall 103 .
[0067] In this embodiment, the process parameters for implanting ions into the substrate 100 of the P-well region 1002 are: ion concentration range is 500E2 ions / cm 2 To 420E3 ions / cm 2 .
[0068] The method for forming lightly doped regions on both sides of the gate structure 102 also includes: using the sidewall 103 as a mask, performing a first ion implantation process in the substrate 100 of the N-well region 1001 to form P-type lightly doped regions 104 in the N-well region 1001 on both sides of the sidewall 103 .
[0069] In this embodiment, the process parameters for implanting ions into the substrate 100 of the N-well region 1001 are: ion concentration range is 220E2 ions / cm 2 Up to 360E3 ions / cm 2 .
[0070] Please refer to Figure 5 A metal nitride layer 106 is formed on the surface of the substrate 100 , the surface of the spacer 103 , and the top surface of the gate structure 102 .
[0071] The method for forming the metal nitride layer 106 is a metal organic chemical vapor deposition process, and the parameters of the metal organic chemical vapor deposition process are: trimethylaluminum (TMA) as an aluminum source, ammonia as a nitrogen source, a temperature of 450° C., and a deposition time of 180 seconds.
[0072] The thickness of the metal nitride layer 106 is in a range of 400 angstroms to 500 angstroms, the stress of the metal nitride layer 106 is in a range of 300 MPa to 600 MPa, and the dielectric constant of the metal nitride is in a range of 8 to 11.5.
[0073] In this embodiment, the metal nitride layer 106 is aluminum nitride, and the thickness of the aluminum nitride is in a range of 400 angstroms to 500 angstroms.
[0074] In other embodiments, the metal nitride layer is.
[0075] The stress range of the aluminum nitride is 300 MPa to 600 MPa. It can be seen that the stress of the aluminum nitride is smaller than the stress of silicon nitride, so that the stress of the first sidewall 107 formed subsequently is reduced, thereby avoiding the wafer from warping or even fragmentation, and ensuring the integrity of the wafer.
[0076] The resistivity range of the aluminum nitride is 10 10 Ω·cm to 10 15 Ω·cm, the thermal conductivity of the aluminum nitride ranges from 170W / m·K to 320W / m·K, and the thermal expansion coefficient of the aluminum nitride is 4.5×10 -6 / K, so that the aluminum nitride can maintain structural stability in a high temperature environment, ensuring the normal operation of ion implantation. Secondly, the chemical stability of aluminum nitride ensures that it will not undergo chemical reactions during the ion implantation process, thereby avoiding adverse effects on the semiconductor film.
[0077] Of course, the present invention does not limit the metal material in the metal nitride layer 106 , and doping of other metals in the metal nitride layer 106 is within the protection scope of the present invention.
[0078] After the step of forming the metal nitride layer 106 , the method further includes: performing a doping treatment on the metal nitride layer 106 to obtain a metal doped layer.
[0079] In this embodiment, the process parameters of the doping treatment are: ammonia as the nitrogen source, the doping temperature is 600 degrees Celsius to 900 degrees Celsius, the pressure is 60mT to 100mT, the doping elements of the doping treatment are scandium, silicon or zirconium, and the dielectric constant of the metal doping layer ranges from 8 to 11.5.
[0080] The dielectric constant of the aluminum nitride is in the range of 8.8 to 8.9. By doping the metal nitride layer 106 and introducing impurity energy levels, the charge distribution and polarization process of the metal nitride layer 106 material are changed, thereby adjusting the dielectric constant and improving the performance of the semiconductor device.
[0081] Please refer to Figure 6 , the metal nitride layer 106 is etched away until the surface of the substrate 100 and the top surface of the gate structure 102 are exposed, so as to form a first sidewall 107 .
[0082] In this embodiment, the process of etching and removing the metal nitride layer 106 is an anisotropic dry etching process, and the process parameters of the dry etching process are that the etching gas is a combination of one or more of H2, CF4, CHF3, CH2F2, C4F8 and Ar, the gas flow rate of the etching gas is 30sccm to 80sccm, the source power is 800W to 1200W, the bias power is 100W to 400W, the etching pressure is 10mTorr to 50mTorr, and the etching time is 30 seconds to 70 seconds.
[0083] After the step of forming the metal nitride layer 106 , the method further includes: performing a second ion implantation process on the substrate 100 using the metal nitride layer 106 as a mask layer to form source / drain regions.
[0084] The method for forming the source / drain region includes: using the first sidewall 107 as a mask, performing a second ion implantation process in the substrate 100 of the P-well region 1002 , and forming N-type source / drain regions 109 on both sides of the first sidewall 107 .
[0085] In this embodiment, the process parameters for implanting ions into the substrate 100 of the P-well region 1002 are: ion concentration range is 500E2 ions / cm 2 To 420E3 ions / cm 2 .
[0086] The method for forming source / drain regions further includes: using the first sidewall 107 as a mask, performing a second ion implantation process in the substrate 100 of the N-well region 1001 to form P-type source / drain regions 108 on both sides of the first sidewall 107 .
[0087] In this embodiment, the process parameters for implanting ions into the substrate 100 of the N-well region 1001 are: ion concentration range is 220E2 ions / cm 2 Up to 360E3 ions / cm 2 .
[0088] Wherein, the ion concentration of the first ion implantation process is less than the ion concentration of the second ion implantation process.
[0089] Accordingly, the present invention further provides a semiconductor structure, further comprising: a substrate 100, wherein the substrate 100 comprises a gate structure 102;
[0090] The first spacer 107 includes: spacers 103 located on both sides of the gate structure 102 , and a metal nitride layer 106 located on the surface of the spacer 103 .
[0091] In this embodiment, the thickness of the metal nitride layer 106 is in a range of 400 angstroms to 500 angstroms, the stress of the metal nitride layer 106 is in a range of 300 MPa to 600 MPa, and the dielectric constant of the metal nitride is in a range of 8 to 11.5.
[0092] In this embodiment, the metal nitride layer 106 is aluminum nitride, the thickness of the aluminum nitride is in a range of 400 angstroms to 500 angstroms, the stress of the aluminum nitride is in a range of 300 MPa to 600 MPa, and the dielectric constant of the aluminum nitride is in a range of 8.8 to 8.9.
[0093] In this embodiment, the spacer 103 includes: a silicon oxide layer 1031 located on the surface of the substrate 100 and the gate structure 102 , and a silicon nitride layer 1032 located on the surface of the silicon oxide layer 1031 .
[0094] In this embodiment, the first spacer 107 includes: a silicon oxide layer 1031 located on the surface of the substrate 100 and the gate structure 102 , a silicon nitride layer 1032 located on the surface of the silicon oxide layer 1031 , and a metal nitride layer 106 located on the surface of the silicon nitride layer 1032 .
[0095] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A method for forming a semiconductor structure, characterized in that: include: Providing a substrate, wherein the substrate includes a gate structure; Forming sidewalls on both sides of the gate structure; Forming a metal nitride layer on the surface of the substrate, the surface of the sidewall, and the top surface of the gate structure; The metal nitride layer is removed by etching until the substrate surface and the top surface of the gate structure are exposed to form a first sidewall.
2. The method for forming a semiconductor structure according to claim 1, wherein: The method for forming the metal nitride layer is a metal organic chemical vapor deposition process, and the parameters of the metal organic chemical vapor deposition process are: a deposition temperature of 400 degrees Celsius to 600 degrees Celsius.
3. The method for forming a semiconductor structure according to claim 2, wherein: The thickness of the metal nitride layer is in a range of 400 angstroms to 500 angstroms, the stress of the metal nitride layer is in a range of 300 MPa to 600 MPa, and the dielectric constant of the metal nitride is in a range of 8 to 11.
5.
4. The method for forming a semiconductor structure according to claim 3, wherein: The metal nitride layer is aluminum nitride, the thickness of the aluminum nitride is in a range of 400 angstroms to 500 angstroms, the stress of the aluminum nitride is in a range of 300 MPa to 600 MPa, and the dielectric constant of the aluminum nitride is in a range of 8.8 to 8.
9.
5. The method for forming a semiconductor structure according to claim 1, wherein: After the step of forming the metal nitride layer, the method further includes: performing a doping treatment on the metal nitride layer to obtain a metal doped layer.
6. The method for forming a semiconductor structure according to claim 5, wherein: The process parameters of the doping treatment are: ammonia as the nitrogen source, the doping temperature is 600 degrees Celsius to 900 degrees Celsius, the pressure is 60mT to 100mT, the doping elements of the doping treatment are scandium, silicon or zirconium, and the dielectric constant of the metal doping layer ranges from 8 to 11.
5.
7. The method for forming a semiconductor structure according to claim 1, wherein: The process of etching and removing the metal nitride layer is a dry etching process. The process parameters of the dry etching process are that the etching gas is a combination of one or more of H2, CF4, CHF3, CH2F2, C4F8 and Ar, the gas flow rate of the etching gas is 30sccm to 80sccm, the source power is 800W to 1200W, the bias power is 100W to 400W, the etching pressure is 10mTorr to 50mTorr, and the etching time is 30 seconds to 70 seconds.
8. The method for forming a semiconductor structure according to claim 1, wherein: The step of forming sidewall spacers on both sides of the gate structure comprises: forming a silicon oxide layer on the surface of the substrate and the gate structure; forming a silicon nitride layer on the surface of the silicon oxide layer; The silicon nitride layer on the substrate is removed by etching until a surface of the silicon oxide layer is exposed.
9. The method for forming a semiconductor structure according to claim 8, wherein: The process for forming the silicon oxide layer is high-temperature furnace tube annealing, and the process parameters of the high-temperature furnace tube annealing are: annealing temperature is 1015 degrees Celsius, and annealing time is 18 seconds. The process for forming the silicon nitride layer is a low-pressure chemical vapor deposition process, and the parameters of the chemical vapor deposition process are: the deposition rate of the silicon nitride layer is 15.3 angstroms per minute to 16.5 angstroms per minute, and the deposition time is 392 seconds.
10. The method for forming a semiconductor structure according to claim 8, wherein: The thickness of the silicon nitride layer ranges from 100 angstroms to 110 angstroms, and the thickness of the silicon oxide layer ranges from 20 angstroms to 25 angstroms.
11. The method for forming a semiconductor structure according to claim 1, wherein: The process of etching and removing the silicon nitride layer is a dry etching process. The process parameters of the dry etching process are that the etching gas is a combination of one or more of CH2F2, CHF3, O2 and He, the gas flow rate of the etching gas is 40sccm to 80sccm, the bias strategy is 50W to 150W, the source power is 600W to 850W, the etching pressure is 30mTorr to 60mTorr, and the etching time is 20 seconds to 40 seconds.
12. The method for forming a semiconductor structure according to claim 1, wherein: After the step of forming the sidewall, the method further comprises: Using the sidewalls as masks, a first ion implantation process is performed on the substrate to form lightly doped regions located on both sides of the gate structure.
13. The method for forming a semiconductor structure according to claim 12, wherein: The process parameters of the first ion implantation treatment are: implantation energy range is 4 kJ to 30 kJ, ion concentration range is 355 E3 ions / cm 2 To 460E4ions / cm 2 , the injection angle is 0 degrees to 45 degrees.
14. The method for forming a semiconductor structure according to claim 1, wherein: After the step of forming the metal nitride layer, the method further comprises: The first sidewall spacer is used as a mask layer to perform a second ion implantation process on the substrate to form a source / drain region.
15. The method for forming a semiconductor structure according to claim 14, wherein: The process parameters of the second ion implantation treatment are an implantation energy range of 6.5 kJ to 20 kJ and an ion concentration range of 200 E3 ions / cm 2 To 280E5ions / cm 2 , the injection angle is 0 degrees to 45 degrees.
16. A semiconductor structure, characterized in that: include: A substrate, wherein the substrate includes a gate structure; A first sidewall spacer includes: sidewalls located on both sides of the gate structure, and a metal nitride layer located on the surface of the sidewall spacer.
17. The semiconductor structure according to claim 16, wherein: The thickness of the metal nitride layer is in a range of 400 angstroms to 500 angstroms, the stress of the metal nitride layer is in a range of 300 MPa to 600 MPa, and the dielectric constant of the metal nitride is in a range of 8 to 11.
5.
18. The semiconductor structure according to claim 17, wherein: The metal nitride layer is aluminum nitride, the thickness of the aluminum nitride is in a range of 400 angstroms to 500 angstroms, the stress of the aluminum nitride is in a range of 300 MPa to 600 MPa, and the dielectric constant of the aluminum nitride is in a range of 8.8 to 8.
9.
19. The semiconductor structure according to claim 16, wherein: The sidewall spacer includes: a silicon oxide layer located on the surface of the substrate and the gate structure, and a silicon nitride layer located on the surface of the silicon oxide layer.
20. The semiconductor structure according to claim 16, wherein: The first sidewall spacer includes: a silicon oxide layer located on the surface of the substrate and the gate structure, a silicon nitride layer located on the surface of the silicon oxide layer, and a metal nitride layer located on the surface of the silicon nitride layer.
Citation Information
Patent Citations
Static random storage unit, through hole structure thereof and production method
CN103280430A
Semiconductor device and forming method thereof
CN108574005A
Integrated chip and manufacturing method thereof
CN112670405A
Semiconductor structure and forming method thereof
CN117832282A
Method for fabricating semiconductor devices
KR1020050073229A