High-toughness Ti (C, N)-based metal ceramic and preparation method thereof
By optimizing the proportion and process of carbide additive phases, Ti(C, N)-based cermet with high strength and toughness is prepared, which solves the problems of different lattice parameters and uneven distribution of additive phases in the prior art, and achieves a higher strength and toughness and comprehensive mechanical properties.
Patent Information
- Application Number
- CN202411249281.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-03
AI Technical Summary
The existing Ti(C, N)-based cermets are prone to collapse or rapid wear during cutting. The main reason is that the difference in lattice parameters caused by the carbide addition phase increases the stress in the grain boundary of the ceramic phase, and the traditional process leads to the added phase. The distribution is uneven and the optimization effect cannot be fully utilized.
By optimizing the molar ratio of the carbide added phase, using high-energy ball milling and protective atmosphere calcining technology, uniform high-entropy carbide powder is prepared to form a ring core phase structure to ensure that the lattice parameter mismatch between the ring phase and the core phase is ≤0.6% , and ensure uniform distribution of the added phases through wet ball milling and vacuum drying.
It significantly improves the strength and toughness of Ti(C, N)-based cermet, improves the material's wear resistance and bending strength, and has good impact toughness. It is suitable for cutting tools and molds and other fields.
Smart Images

Figure CN119061303A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal ceramic materials, and in particular to a high-strength and toughness Ti (C, N)-based metal ceramic and a preparation method thereof. Background Art
[0002] Ti(C, N)-based cermets have the advantages of high red hardness, high strength, and low friction coefficient with non-ferrous metals. They are high-speed cutting tools and hot working die materials for metal processing such as cast iron and steel. At present, the wettability of the ceramic phase and the binder phase of Ti(C, N)-based cermets is poor, resulting in low bonding strength of the ceramic-metal interface, low toughness of the cermets, and easy chipping of the tool during cutting. In the prior art, in order to improve the service performance of Ti(C, N)-based cermet tools, some additive phases are usually introduced into the material system to regulate the comprehensive performance of the material. According to their efficacy, they can be mainly divided into three categories, namely (1) tungsten carbide and molybdenum carbide, which can significantly optimize the wettability of the ceramic phase and the binder phase Co / Ni and improve the grain interface bonding strength; (2) tantalum carbide and niobium carbide, which improve the high temperature creep resistance of cermets; (3) zirconium carbide and vanadium carbide, which refine the grains of cermets and improve the material's oxidation resistance. At present, the content of the above additives is combined based on empiricism. Generally speaking, 15-25 wt% WC and / or Mo2C, 3-5wt% TaC and / or NbC, 1-2wt% ZrC and / or VC, etc. are usually added. After sintering, a typical ring-core phase structure will be formed in the Ti(C, N)-based cermet structure through the dissolution-precipitation process. The ring phase is a solid solution composed of (Ti, W, Mo, Ta, Nb, Zr, V)(C,N), and the core phase is Ti(C,N). For this reason, there is a certain lattice difference in the interface of the ring-core phase, which reduces the fracture energy of the ring-core phase grains. As shown in the literature (see Ceramics International 44 (2018) 19113–19122, Figure 7), the influence of different solid solution atoms on the lattice parameters of Ti(C, N) was quantitatively characterized. It also confirmed that low lattice mismatch at the ring-core interface can effectively improve the mechanical properties of Ti(C, N)-based cermets.
[0003] In the prior art, Ti(C, N)-based cermets mainly improve the interface strength between the ceramic phase and the metal phase and improve the sintering density and organizational uniformity of the material by adding a certain amount of carbides (such as tungsten carbide, molybdenum carbide, tantalum carbide, niobium carbide, etc.). However, due to the addition of other carbide additives, through subsequent high-temperature liquid phase sintering, the cermet will form a typical ring-core phase structure, but not much attention has been paid to the influence of the lattice mismatch of the ring-core phase on the service performance of the material. Therefore, there are mainly the following two problems.
[0004] Question 1: Although carbides are added to help control the sintering density and uniformity of metal ceramics, the solid solution of carbides into the Ti(C, N) lattice will cause the lattice to expand or shrink, resulting in a large difference in the lattice parameters of the ring phase and the core phase, increasing the stress within the grain boundary of the ceramic phase, resulting in a decrease in the energy consumed by the fracture of the ceramic phase during the failure process of the material, which is manifested as the Ti(C, N)-based metal ceramics being prone to chipping or rapid wear during the cutting process.
[0005] Question 2: Conventional additive phases are usually added in the form of multiple carbides at the same time, and then a mixed powder is obtained through a long period of wet grinding. This process will result in uneven distribution of the additive phases, resulting in uneven composition of the ring phase formed in the early stage, and cannot fully exert the effect of the optimized additive phase components on reducing the lattice mismatch of the material. Summary of the invention
[0006] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a high-strength and toughness Ti (C, N) based cermet and a preparation method thereof.
[0007] In order to achieve the above-mentioned object, a high-strength and toughness Ti(C, N)-based cermet and a preparation method thereof are provided, wherein the hard phase microstructure of the Ti(C, N)-based cermet is a ring-core phase, and the ring-core phase is composed of a core phase and a ring phase covering the core phase; wherein the lattice parameter mismatch between the ring phase and the core phase is ≤0.6%; The composition of the core phase is Ti(C, N), the composition of the ring phase is (Ti, M) (C, N) solid solution, and the M includes at least one of W and Mo, at least one of Ta and Nb, V, and Zr.
[0008] Preferably, the binder phase of the Ti(C,N)-based cermet is composed of at least one of iron, cobalt and nickel.
[0009] The invention provides a preparation method of a high-strength and tough Ti (C, N)-based cermet, comprising the following steps: step 1: preparing according to the molar ratio of a carbide additive phase, mixing the powders and then wet ball milling, wherein the ball milling medium is an organic solvent, the ball-to-material ratio is 12-20:1, the ball milling time is 12-60 hours, and the ball milling speed is 120-300 r / min; then the ball-milled powder is vacuum dried, and after drying, high-temperature calcination is performed to form a single-phase high-entropy carbide powder from the carbide mixed powder. The calcination temperature is 1600-2000°C, and the calcination atmosphere is high-purity argon gas with a purity better than 99.999%; step 2: prepare Ti(C, N) powder, the high entropy carbide powder synthesized in step 1, the binder phase powder and the carbon black powder according to the designed proportion for wet ball milling, the ball-to-material ratio is 5-8:1, the ball milling speed is 80-200r / min, and the ball milling time is 24-60h; after the ball milling is completed, the mixed powder is vacuum dried to obtain a Ti(C, N)-based metal ceramic mixture; step 3: dry the mixture, sieve the undersize obtained by sieving, and press-form to obtain a compact; step 4: degrease and sinter the compact to obtain a Ti(C, N)-based metal ceramic.
[0010] Preferably, in step one, the carbide additive phase includes four components: at least one of WC and Mo2C, at least one of TaC and NbC, VC, and ZrC, and the molar ratio of the four components of the carbide additive phase is 1: 0.2-0.3: 0.1-0.15: 0.05-0.1.
[0011] Preferably, in step 2, the raw materials include the following components in parts by mass: 40-60 parts of Ti(C,N) powder; 20-35 parts by total mass fraction of high entropy carbide additive phase; 12-20 parts of binder phase powder, and 0.1-0.5 parts of carbon black.
[0012] Preferably, the average particle size of the Ti(C,N) powder is 0.5-5.0 μm, the average particle size of the high entropy carbide powder is 0.2-3.0 μm, the average particle size of the binder phase powder is 2-20 μm, and the average particle size of the carbon black is 0.1-20 μm.
[0013] Preferably, in step three, the pressing pressure is 100-200 MPa.
[0014] Preferably, the degreasing is carried out in a vacuum environment, the degreasing temperature is 300-500° C., and the degreasing time is 2-5 hours.
[0015] Preferably, in step four, the sintering process is to first heat the temperature to 1000-1200°C in a vacuum environment, keep it warm for 1-3 hours, then introduce a mixed gas of nitrogen and argon, control the gas pressure in the sintering furnace to 1×102-5×103 Pa, and simultaneously heat the temperature to 1220-1300°C, keep it warm for 3-5 hours, and then introduce high-purity argon to make the pressure 1-5MPa, and heat to 1430-1500°C at a rate of ≤5-8°C / min, and keep it warm for 1-3 hours.
[0016] Preferably, in the mixed gas of nitrogen and argon, the flow ratio of nitrogen to argon is 1-5:9-5.
[0017] Compared with the prior art, the beneficial effects of the present invention are: The present invention is based on the influence of carbide components on the Ti (C, N) lattice, optimizes the proportion of added phase components, so that the internal stress of the metal ceramic ring core phase interface after sintering is less than 0.60%. At the same time, the carbide added phase is pre-treated to be homogenized, so that the ring core phase components can be accurately controlled during the sintering process, and has the following significant technical advantages.
[0018] The fracture energy of the Ti(C,N)-based metal ceramic ring core phase grains is effectively improved, making the metal ceramic have higher strength and toughness.
[0019] High-entropy carbide ceramic powder with uniform composition was artificially prepared by high-energy ball milling and protective atmosphere calcination. By replacing the traditional multi-component addition method with the homogenized carbide additional phase powder, the composition of the ring core phase after sintering was made more uniform, further exerting the above-mentioned optimized carbide additional phase composition and improving the comprehensive mechanical properties of the metal ceramic material.
[0020] The Ti(C,N)-based cermet prepared by this method has excellent comprehensive properties, and the tool products have strong resistance to wear and chipping. The material has high bending strength (better than 2300MPa), good impact toughness (better than 2.30 J / cm2), high Rockwell hardness (better than 92.0), and the lattice mismatch of the cermet is lower than 0.60%. The cermet material can be widely used in bearing materials, cutting tools, mold materials and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required to be used in the embodiments are briefly introduced below.
[0022] Figure 1 The powder morphology of the carbide added phase by high energy ball milling of the present invention.
[0023] Figure 2This is the morphology of the high entropy carbide powder after calcination at 1800°C for 1 hour.
[0024] Figure 3 The SEM microstructure morphology of the Ti(C,N)-based cermet with low interfacial stress in Example 1 of the present invention.
[0025] Figure 4 XRD spectra of the metal ceramic materials prepared in Examples 1-3 and Comparative Examples 1-3 of the present invention Figure 5 It is a bending strength curve diagram of the metal ceramic materials prepared in Examples 1-3 of the present invention and Comparative Examples 1-2.
[0026] Figure 1 , Figure 2 The carbides include four components, the first type is tungsten carbide and molybdenum carbide, the second type is tantalum carbide, the third type is vanadium carbide, and the fourth type is zirconium carbide. The molar ratio of the above four types of carbides is 1:0.2:0.12:0.08. The powder ball milling ratio is 15:1, the ball milling time is 24h; the high temperature calcination temperature is 1800℃, and the calcination time is 3h. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0028] Example 1 Composition: 45Ti(C,N)-35(W, Mo,Ta, V, Zr)C-19.5Ni-0.5C metal ceramic, wherein the atomic ratio of (W+Mo):Ta:V:Zr=1:0.2:0.1:0.05.
[0029] The mass fraction of the metal ceramic component is 45 parts of Ti(C, N), 35 parts of high entropy carbide powder (W, Mo, Ta, V, Zr)C, 19.5 parts of binder phase and 0.5 parts of carbon black. The average particle size of Ti(C, N) is 1.0 micron, the particle size of high entropy carbide powder is 2.0 micron, and the particle size of carbon black is 1.0 micron.
[0030] The preparation steps of the metal ceramic are as follows: (1) weighing WC, Mo2C, TaC, VC and ZrC powders are placed in a ball mill, and anhydrous ethanol is added until it exceeds the surface of the balls and the powders; the ball mill barrel is planetarily milled, with a ball-to-material ratio of 15:1, a rotation speed of 200 r / min, and a ball milling time of 24 hours; then the powder is vacuum dried at a drying temperature of 60°C and a drying time of 12 hours; then the dried powder is calcined, the protective atmosphere is high-purity argon, the calcination temperature is 1800°C, and the calcination time is 3 hours. (2) The weighed Ti(C,N) powder, synthesized high entropy carbide powder, metal binder phase powder and carbon black are placed in a ball mill, and anhydrous ethanol is added until it does not exceed the surface of the balls and powder; the ball mill barrel is subjected to roller milling, with a ball-to-material ratio of 8:1, a rotation speed of 100 r / min, and a ball milling time of 30 h; (4) The powder is then passed through a 200-mesh sieve and cold pressed at a pressing pressure of 200 MPa for 10 s; (5) The compact is then placed in a debinding and sintering integrated furnace for debinding and sintering, with a vacuum debinding temperature of 500 °C for 2 h and a solid phase holding temperature of 1200 °C for 2 h; a mixed gas of nitrogen and argon is then introduced, while a vacuum pump continues to evacuate the gas, and the vacuum pump's stable exhaust pressure is adjusted to 1×103 Pa. The flow ratio of nitrogen and argon is 2:8, and the insulation temperature is 1300°C for 2 hours. Then the temperature is increased at a rate of 5°C / min, and high-purity argon is introduced at the same time to make the gas pressure in the furnace 2MPa. The final sintering temperature is 1450°C, and it is kept for 1 hour to obtain metal ceramics.
[0031] The hardness of the metal ceramic is 92.8HRA, the bending strength is 2450MPa, and the impact toughness is 2.42 J / cm2. The interface lattice mismatch of the Ti(C,N)-based metal ceramic ring core is 0.28%, and the tool has good application prospects.
[0032] Example 2 Composition: 50Ti(C,N)-30(W, Mo,Ta, Nb,V, Zr)C-19.8Ni-0.2C metal ceramic, among which the atomic ratio of (W+Mo):(Ta+Nb):V:Zr = 1:0.25:0.12:0.07.
[0033] The mass fraction of the metal ceramic component is 50 parts of Ti(C, N), 30 parts of high entropy carbide powder (W, Mo, Ta, V, Zr)C, 19.8 parts of binder phase and 0.2 parts of carbon black. The average particle size of Ti(C, N) is 3.0 microns, the particle size of high entropy carbide powder is 1.0 microns, and the particle size of carbon black is 10.0 microns.
[0034] The preparation steps of the metal ceramic are as follows: (1) weighing WC, Mo2C, TaC, NbC, VC and ZrC powders are placed in a ball mill, and anhydrous ethanol is added until it exceeds the surface of the balls and the powders; the ball mill barrel is planetarily milled, with a ball-to-material ratio of 20:1, a rotation speed of 250 r / min, and a ball milling time of 20 hours; then the powder is vacuum dried at a drying temperature of 60°C and a drying time of 12 hours; then the dried powder is calcined, the protective atmosphere is high-purity argon, the calcination temperature is 1900°C, and the calcination time is 2 hours. (2) The weighed Ti(C,N) powder, synthesized high entropy carbide powder, metal binder phase powder and carbon black are placed in a ball mill, and anhydrous ethanol is added until it does not exceed the surface of the balls and powder; the ball mill is subjected to roller milling with a ball-to-material ratio of 6:1, a rotation speed of 200 r / min, and a ball milling time of 48 h; (4) The powder is then passed through a 200-mesh sieve and cold pressed at a pressing pressure of 200 MPa for 10 s; (5) The compact is then placed in a debinding and sintering integrated furnace for debinding and sintering, with a vacuum debinding temperature of 500 °C for 2 h and a solid phase holding temperature of 1200 °C for 2 h; a mixed gas of nitrogen and argon is then introduced, while a vacuum pump continues to evacuate the gas, and the vacuum pump's stable exhaust pressure is adjusted to 5×103 Pa. The flow ratio of nitrogen and argon is 2:8, and the insulation temperature is 1300°C for 2 hours. Then the temperature is increased at a rate of 5°C / min, and high-purity argon is introduced at the same time to make the gas pressure in the furnace 5MPa. The final sintering temperature is 1480°C, and the temperature is maintained for 1 hour to obtain metal ceramics.
[0035] The hardness of the metal ceramic is 92.5HRA, the bending strength is 2350MPa, and the impact toughness is 2.35 J / cm2. The lattice mismatch degree of the Ti(C,N)-based metal ceramic ring core interface is 0.35%, and the Ti(C,N) tool has good application prospects.
[0036] Example 3 Composition: 58Ti(C,N)-26(W, Mo,Ta, Nb,V, Zr)C-15.8Ni-0.2C metal ceramic, among which the atomic ratio of (W+Mo):(Ta+Nb):V:Zr = 1:0.3:0.15:0.09.
[0037] The mass fraction of the metal ceramic component is 58 parts of Ti(C, N), 26 parts of high entropy carbide powder (W, Mo, Ta, V, Zr)C, 15.8 parts of binder phase and 0.2 parts of carbon black. The average particle size of Ti(C, N) is 5.0 microns, the particle size of high entropy carbide powder is 3.0 microns, and the particle size of carbon black is 20.0 microns.
[0038] The preparation steps of the metal ceramic are as follows: (1) weighing WC, Mo2C, TaC, NbC, VC and ZrC powders in a ball mill, adding anhydrous ethanol until the powders are above the surface of the balls and the powders; planetary milling the ball mill with a ball-to-material ratio of 20:1, a rotation speed of 300 r / min and a ball milling time of 20 h; then vacuum drying the powder at a drying temperature of 80°C and a drying time of 12 h; then calcining the dried powder with a protective atmosphere of high-purity argon gas at a calcination temperature of 2000°C and a calcination time of 3 h. (2) The weighed Ti(C,N) powder, synthesized high entropy carbide powder, metal binder phase powder and carbon black are placed in a ball mill, and anhydrous ethanol is added until it does not exceed the surface of the balls and powder; the ball mill barrel is subjected to roller milling, with a ball-to-material ratio of 5:1, a rotation speed of 100 r / min, and a ball milling time of 60 h; (4) The powder is then passed through a 200-mesh sieve and cold pressed at a pressing pressure of 200 MPa for 10 s; (5) The compact is then placed in a debinding and sintering integrated furnace for debinding and sintering, with a vacuum debinding temperature of 500 °C for 3 h and a solid phase holding temperature of 1200 °C for 3 h; a mixed gas of nitrogen and argon is then introduced, while a vacuum pump continues to evacuate the gas, and the vacuum pump's stable exhaust pressure is adjusted to 5×103 Pa. The flow ratio of nitrogen and argon is 3:7, and the insulation temperature is 1300°C for 2 hours. Then the temperature is increased at a rate of 5°C / min, and high-purity argon is introduced at the same time to make the gas pressure in the furnace 5MPa. The final sintering temperature is 1500°C, and the temperature is maintained for 2 hours to obtain metal ceramics.
[0039] The hardness of the metal ceramic is 92.1HRA, the bending strength is 2250MPa, and the impact toughness is 2.30 J / cm2. The lattice mismatch degree of the Ti(C,N)-based metal ceramic ring core interface is 0.52%, and the Ti(C,N) tool has good application prospects.
[0040] Comparative Example 1 The other conditions are the same as those in Example 1, except that the carbide additive phase powder is added directly and separately without going through step 1.
[0041] The hardness of the metal ceramic is 91.8HRA, the bending strength is 2160MPa, and the impact toughness is 2.12 J / cm2. The interface lattice mismatch of the Ti(C,N)-based metal ceramic ring core is 0.85%, and the tool is prone to chipping.
[0042] Comparative Example 2 The other conditions are the same as those in Example 1, and there are only three types of carbide added phase powders: A, B, and C.
[0043] The hardness of the metal ceramic is 92.1HRA, the bending strength is 1980MPa, and the impact toughness is 2.21 J / cm2. The interface lattice mismatch of the Ti(C,N)-based metal ceramic ring core is 1.30%.
[0044] Comparative Example 3 The other conditions were the same as those in Example 1, except that high-pressure argon gas was not charged in the preparation step 4, and the pressure of the charged argon gas was only 0.5 MPa.
[0045] The hardness of the metal ceramic is 92.1HRA, the bending strength is 2150MPa, and the impact toughness is 2.11 J / cm2. The interface lattice mismatch of the Ti(C,N)-based metal ceramic ring core is 0.75%.
[0046] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.
Claims
1. A high-strength and tough Ti(C, N)-based cermet, characterized in that: The hard phase microstructure of the Ti(C,N)-based cermet is a ring-core phase, which is composed of a core phase and a ring phase covering the core phase; wherein the mismatch between the lattice parameter of the ring phase and the lattice parameter of the core phase is ≤0.6%; The composition of the core phase is Ti(C, N), the composition of the ring phase is (Ti, M) (C, N) solid solution, and the M includes at least one of W and Mo, at least one of Ta and Nb, V, and Zr.
2. A high-strength and tough Ti(C, N)-based cermet according to claim 1, characterized in that: The binder phase of the Ti(C,N)-based cermet is composed of at least one of iron, cobalt and nickel.
3. A method for preparing a high-strength and tough Ti(C, N)-based cermet according to any one of claims 1-2, characterized in that: The following steps are involved: Step 1: According to the molar ratio of the carbide additive phase, the powder is prepared and mixed, and then wet ball milling is performed, the ball milling medium is an organic solvent, the ball-to-material ratio is 12-20:1, the ball milling time is 12-60 hours, and the ball milling speed is 120-300r / min; then the ball-milled powder is vacuum dried, and after drying, high-temperature calcination is performed to form the above-mentioned carbide mixed powder into a single-phase high-entropy carbide powder. The calcination temperature is 1600-2000°C, and the calcination atmosphere is high-purity argon gas with a purity better than 99.999%; step 2: prepare Ti(C, N) powder, the high entropy carbide powder synthesized in step 1, the binder phase powder and the carbon black powder according to the designed proportion for wet ball milling, the ball-to-material ratio is 5-8:1, the ball milling speed is 80-200r / min, and the ball milling time is 24-60h; after the ball milling is completed, the mixed powder is vacuum dried to obtain a Ti(C, N)-based metal ceramic mixture; step 3: dry the mixture, sieve the undersize obtained by sieving, and press-form to obtain a compact; step 4: degrease and sinter the compact to obtain a Ti(C, N)-based metal ceramic.
4. A high-strength and toughness Ti(C, N)-based cermet and a preparation method thereof according to claim 3, characterized in that: In step 1, the carbide additive phase includes four components: at least one of WC and Mo2C, at least one of TaC and NbC, VC, and ZrC. The molar ratio of the four components of the carbide additive phase is 1: 0.2-0.3: 0.1-0.15: 0.05-0.
1.
5. A high-strength and toughness Ti(C, N)-based cermet and a preparation method thereof according to claim 3, characterized in that: In step 2, the raw materials include the following components by weight: 40-60 parts of Ti(C,N) powder; 20-35 parts by total weight fraction of high entropy carbide additive phase; 12-20 parts of binder phase powder and 0.1-0.5 parts of carbon black.
6. A high-strength and toughness Ti(C, N)-based cermet and a preparation method thereof according to claim 5, characterized in that: The average particle size of the Ti(C,N) powder is 0.5-5.0 μm, the average particle size of the high entropy carbide powder is 0.2-3.0 μm, the average particle size of the binder phase powder is 2-20 μm, and the average particle size of the carbon black is 0.1-20 μm.
7. A high-strength and toughness Ti(C, N)-based cermet and a preparation method thereof according to claim 3, characterized in that: In step three, the pressure of the pressing molding is 100-200 MPa.
8. A high-strength and toughness Ti(C, N)-based cermet and a preparation method thereof according to claim 3, characterized in that: In step 4, the degreasing is carried out in a vacuum environment, the degreasing temperature is 300-500° C., and the degreasing time is 2-5 hours.
9. A high-strength and toughness Ti(C, N)-based cermet and a preparation method thereof according to claim 3, characterized in that: In step 4, the sintering process is to first heat the temperature to 1000-1200°C in a vacuum environment, keep it warm for 1-3 hours, then introduce a mixed gas of nitrogen and argon, control the gas pressure in the sintering furnace to 1×102-5×103 Pa, and heat it to 1220-1300°C at the same time, keep it warm for 3-5 hours, and then introduce high-purity argon to make the pressure 1-5MPa, and heat it to 1430-1500°C at a rate of ≤5-8°C / min, and keep it warm for 1-3 hours.
10. A high-strength and toughness Ti(C, N)-based cermet and a preparation method thereof according to claim 3, characterized in that: In the mixed gas of nitrogen and argon, the flow ratio of nitrogen to argon is 1-5:9-5.
Citation Information
Cited By
Preparation method of high-entropy carbide-based metal ceramic
CN119506638A
Metal ceramic composite material with synergic toughness improvement, preparation method and application
CN121575287A
Metal ceramic composite material with complete core ring structure, preparation method and application
CN121589289A
Complex-phase Ti (C, N)-based ceramic material with double-solid-solution microstructure and preparation method of complex-phase Ti (C, N)-based ceramic material
CN121895048A