Preparation method of novel silicon-carbon surface passivation layer

By oxidizing and doping the silicon carbon negative electrode material with phosphoric acid solution in lithium-ion batteries, the SiO2 passivation layer is formed, which solves the side reaction problem of silicon negative electrode material with electrolyte in lithium-ion batteries, and improves the conductivity and Cycle stability significantly improves the performance of lithium-ion batteries.

CN118969985APending Publication Date: 2024-11-15XUANCHENG SILIKO NEW MATERIALS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411014675.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The side reaction between the silicon negative electrode material of lithium batteries and the electrolyte during the deintercalation process of lithium-ion batteries has not been effectively solved, which limits its application in lithium-ion batteries.

Method used

The silicon carbon negative electrode material deposited in porous carbon is oxidized to form a SiO2 layer, and phosphorus doping is performed during high-temperature calcination to form n-type doping to improve conductivity and cycling stability.

Benefits of technology

Through phosphoric acid treatment, the formed SiO2 passivation layer effectively prevents the volume expansion and contraction of the silicon material, improves the cyclic stability and conductivity of the silicon carbon negative electrode material, and significantly improves the performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969985A_ABST
    Figure CN118969985A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of a silicon negative electrode material of a lithium battery, in particular to a preparation method of a novel silicon-carbon surface passivation layer. The method comprises the following steps: S1, preparing a phosphoric acid solution in which the proportion of phosphoric acid to silicon carbon is 1-20wt%; s2, adding a silicon-carbon negative electrode material formed by depositing silicon in pores of the porous carbon into a phosphoric acid solution with the solid content of 3-40%, and uniformly stirring and mixing to form a mixed solution; s3, carrying out centrifugal separation on the mixed solution; s4, adding into a rotary furnace, and roasting for 1-5 hours at the temperature of 400-900 DEG C in an inert gas atmosphere; and S5, cooling and discharging. According to the novel preparation method of the silicon-carbon surface passivation layer, a silicon-carbon negative electrode material formed by depositing silicon in pores of porous carbon is oxidized into a SiO2 layer by a phosphoric acid solution, so that side reaction of silicon and electrolyte in a battery is avoided, residual phosphoric acid is doped with silicon during high-temperature roasting to form n-type doping, and after phosphorus doping, the silicon-carbon surface passivation layer is formed. And the conductivity of silicon is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of silicon negative electrode materials for lithium batteries, and in particular to a method for preparing a novel silicon-carbon surface passivation layer. Background Art

[0002] At present, new energy vehicles are rapidly popularizing and are gradually replacing fuel vehicles. However, the low energy density of lithium batteries is an important reason that limits their rapid promotion. The main problem is that the graphite negative electrode has a low gram capacity. Silicon negative electrodes have become the new favorite of the industry due to their high theoretical capacity, but due to the large volume effect of silicon, their application is greatly restricted. The volume expansion is too large and it cannot be used in lithium-ion batteries. In response to this, the academic community mentioned in "High-performance lithium-ion anodes using a hierarchical bottom-up approach" that SiH4 is deposited in porous carbon to alleviate its large volume effect during lithium deintercalation. However, the large side reaction of silicon negative electrodes with electrolytes during lithium deintercalation has not been solved.

[0003] The present invention aims at solving this problem and urgently needs a novel method for preparing a silicon-carbon surface passivation layer to solve the deficiencies of the prior art. Summary of the invention

[0004] The purpose of the present invention is to provide a novel method for preparing a silicon-carbon surface passivation layer to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides a method for preparing a novel silicon-carbon surface passivation layer, comprising the following steps:

[0006] S1. Prepare a phosphoric acid solution in which the phosphoric acid ratio is 1-20wt% of the silicon-carbon ratio;

[0007] S2, adding the silicon-carbon negative electrode material formed by depositing silicon in the pores of the porous carbon into a phosphoric acid solution with a solid content of 3-40% and stirring and mixing evenly to form a mixed solution;

[0008] S3, centrifuging the mixed solution;

[0009] S4, adding into a rotary kiln, and calcining at 400-900°C for 1-5h under an inert gas atmosphere;

[0010] S5, cooling and discharging.

[0011] As a further improvement of the technical solution, in S1, phosphoric acid is configured to account for 1 wt% of the silicon-carbon ratio.

[0012] As a further improvement of the technical solution, in S1, phosphoric acid is configured to account for 4 wt% of the silicon-carbon ratio.

[0013] As a further improvement of the technical solution, in S1, phosphoric acid is configured to account for 12 wt % of silicon-carbon ratio.

[0014] As a further improvement of the technical solution, in S1, the phosphoric acid is configured to have a silicon-carbon ratio of 20wt%.

[0015] As a further improvement of the technical solution, in S2, the silicon-carbon negative electrode material formed by depositing silicon in the pores of the porous carbon is added to the phosphoric acid solution, and the solid content is 20%.

[0016] As a further improvement of the technical solution, in S2, the silicon-carbon negative electrode material formed by depositing silicon in the pores of the porous carbon is added to the phosphoric acid solution, and the solid content is 40%.

[0017] As a further improvement of the technical solution, in S4, the calcination temperature is 400° C. and the time is 1 hour.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. In the preparation method of the new silicon-carbon surface passivation layer, the silicon-carbon negative electrode material formed by depositing silicon in the pores of the porous carbon is oxidized into a SiO2 layer by a phosphoric acid solution to avoid side reactions between silicon and the electrolyte in the battery. The residual phosphoric acid dopes the silicon during high-temperature calcination to form n-type doping. After phosphorus doping, the conductivity of silicon is improved, thereby improving its rate performance.

[0020] 2. In the preparation method of the new silicon-carbon surface passivation layer, as the proportion of phosphoric acid increases, the cycle stability of the passivated silicon-carbon negative electrode material gradually increases, but its conductivity shows a trend of first increasing and then decreasing. This is due to the excess residual phosphoric acid, and the phosphate and pyrophosphate formed during high-temperature roasting; phosphate or pyrophosphate, which is conducive to the construction of a stable solid electrolyte interface layer, thereby protecting the silicon-carbon negative electrode material, reducing the decomposition of the electrolyte and maintaining good electrochemical contact. Among them, when the proportion of phosphoric acid reaches 12wt%, the 30-cycle capacity retention rate reaches 96%, showing excellent cycle stability. This is due to the SiO2 passivation layer formed during the phosphoric acid treatment process, which can effectively prevent the volume expansion and contraction of the silicon material during the charge and discharge process, thereby reducing the shedding of active substances and the destruction of the electrode structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a schematic diagram of the structure of Example 1 of the present invention. DETAILED DESCRIPTION

[0022] The following will be combined with the accompanying drawings in the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0023] The embodiment of the present invention provides a method for preparing a novel silicon-carbon surface passivation layer, and the specific steps are as follows:

[0024] Step 1, preparing a phosphoric acid solution with a phosphoric acid to silicon carbon ratio of 1-20wt%;

[0025] Step 2: Add the silicon-carbon negative electrode material formed by depositing silicon in the pores of the porous carbon into a phosphoric acid solution with a solid content of 3-40% and stir for a period of time to mix evenly to form a mixed solution. The exposed nano-silicon layer on the surface of the porous carbon is oxidized by phosphoric acid to form a SiO2 layer.

[0026] Step 3, centrifuging the mixed solution;

[0027] Step 4: Add the silicon to a rotary kiln and bake it at 400-900° C. for 1-5 hours in an inert gas atmosphere; the residual phosphoric acid dopes the silicon during high-temperature baking to form n-type doping.

[0028] Step 5: Cool and discharge.

[0029] In the present invention, the silicon-carbon negative electrode material formed by depositing silicon in the pores of the porous carbon is oxidized into a SiO2 layer by a phosphoric acid solution, thereby avoiding a side reaction between silicon and the electrolyte in the battery. The residual phosphoric acid dopes the silicon during high-temperature calcination to form an n-type doping. After phosphorus doping, the conductivity of silicon is improved, thereby improving its rate performance. Figure 1 It can be seen that there is a SiO2 layer on the surface of the silicon-carbon negative electrode, and the silicon in contact with the SiO2 layer is doped with phosphorus.

[0030] Example 1

[0031] Step 1, preparing a phosphoric acid solution in which the phosphoric acid ratio is 1wt% of silicon-carbon;

[0032] Step 2: Add the silicon-carbon negative electrode material formed by depositing silicon in the pores of the porous carbon into a phosphoric acid solution with a solid content of 20% and stir for a period of time to mix evenly to form a mixed solution;

[0033] Step 3, centrifuging the mixed solution;

[0034] Step 4: Add the mixture into a rotary kiln and calcine it at 400°C for 1 hour under an inert gas atmosphere;

[0035] Step 5: Cool and discharge.

[0036] Example 2

[0037] Step 1, preparing a phosphoric acid solution in which the phosphoric acid ratio is 4wt% of silicon-carbon;

[0038] Step 2: Add the silicon-carbon negative electrode material formed by depositing silicon in the pores of the porous carbon into a phosphoric acid solution with a solid content of 20% and stir for a period of time to mix evenly to form a mixed solution;

[0039] Step 3, centrifuging the mixed solution;

[0040] Step 4: Add the mixture into a rotary kiln and calcine it at 400°C for 1 hour under an inert gas atmosphere;

[0041] Step 5: Cool and discharge.

[0042] Example 3

[0043] Step 1, preparing a phosphoric acid solution with a phosphoric acid to silicon carbon ratio of 12wt%;

[0044] Step 2: Add the silicon-carbon negative electrode material formed by depositing silicon in the pores of the porous carbon into a phosphoric acid solution with a solid content of 20% and stir for a period of time to mix evenly to form a mixed solution;

[0045] Step 3, centrifuging the mixed solution;

[0046] Step 4: Add the mixture into a rotary kiln and calcine it at 400°C for 1 hour under an inert gas atmosphere;

[0047] Step 5: Cool and discharge.

[0048] Example 4

[0049] Step 1, preparing a phosphoric acid solution in which the phosphoric acid ratio is 20wt% of silicon-carbon ratio;

[0050] Step 2: Add the silicon-carbon negative electrode material formed by depositing silicon in the pores of the porous carbon into a phosphoric acid solution with a solid content of 40% and stir for a period of time to mix evenly to form a mixed solution;

[0051] Step 3, centrifuging the mixed solution;

[0052] Step 4: Add the mixture into a rotary kiln and calcine it at 400°C for 1 hour under an inert gas atmosphere;

[0053] Step 5: Cool and discharge.

[0054] Table 1

[0055]

[0056]

[0057] Table 2

[0058] Phosphoric acid to silicon carbon ratio (%) <![CDATA[Conductivity (S·cm -1 )]]> 30-cycle capacity retention rate (%) Example 1 1 0.91 84 Example 2 4 2.13 91 Example 3 12 0.41 96 Example 4 20 0.23 90

[0059] According to Table 2, in Examples 1-4, as the proportion of phosphoric acid increases, the cycle stability of the passivated silicon-carbon negative electrode material gradually increases, but its conductivity shows a trend of first increasing and then decreasing. This is due to the excess residual phosphoric acid, and the phosphate and pyrophosphate formed during high-temperature roasting; phosphate or pyrophosphate, which is conducive to building a stable solid electrolyte interface layer, thereby protecting the silicon-carbon negative electrode material, reducing the decomposition of the electrolyte and maintaining good electrochemical contact. In Example 3, when the proportion of phosphoric acid reaches 12wt%, the 30-cycle capacity retention rate reaches 96%, showing excellent cycle stability. This is due to the SiO2 passivation layer formed during the phosphoric acid treatment, which can effectively prevent the volume expansion and contraction of the silicon material during the charge and discharge process, thereby reducing the shedding of active substances and the destruction of the electrode structure.

[0060] The novel method for preparing the silicon-carbon surface passivation layer provided by the present invention can significantly improve the cycle stability and initial efficiency of the silicon-carbon negative electrode material without sacrificing the conductivity by adjusting the proportion of the phosphoric acid solution, which is of great significance for the development of high-performance lithium-ion batteries.

[0061] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a novel silicon-carbon surface passivation layer, characterized in that: The following steps are involved: S1. Prepare a phosphoric acid solution in which the phosphoric acid ratio is 1-20wt% of the silicon-carbon ratio; S2, adding the silicon-carbon negative electrode material formed by depositing silicon in the pores of the porous carbon into a phosphoric acid solution with a solid content of 3-40% and stirring and mixing evenly to form a mixed solution; S3, centrifuging the mixed solution; S4, adding into a rotary kiln, and calcining at 400-900°C for 1-5h under an inert gas atmosphere; S5, cooling and discharging.

2. The method for preparing the novel silicon-carbon surface passivation layer according to claim 1, characterized in that: In the S1, phosphoric acid is configured to account for 1 wt% of the silicon-carbon ratio.

3. The method for preparing the novel silicon-carbon surface passivation layer according to claim 1, characterized in that: In the S1, phosphoric acid is configured to account for 4 wt % of the silicon-carbon ratio.

4. The method for preparing the novel silicon-carbon surface passivation layer according to claim 1, characterized in that: In the S1, phosphoric acid is configured to account for 12 wt % of the silicon-carbon ratio.

5. The method for preparing the novel silicon-carbon surface passivation layer according to claim 1, characterized in that: In the S1, phosphoric acid is configured to account for 20wt% of the silicon-carbon ratio.

6. The method for preparing the novel silicon-carbon surface passivation layer according to any one of claims 2 to 4, characterized in that: In S2, the silicon-carbon negative electrode material formed by depositing silicon in the pores of the porous carbon is added into the phosphoric acid solution, and the solid content is 20%.

7. The method for preparing the novel silicon-carbon surface passivation layer according to claim 5, characterized in that: In S2, the silicon-carbon negative electrode material formed by depositing silicon in the pores of the porous carbon is added into the phosphoric acid solution, and the solid content is 40%.

8. The method for preparing the novel silicon-carbon surface passivation layer according to claim 1, characterized in that: In the step S4, the calcination temperature is 400° C. and the calcination time is 1 h.

Citation Information

Cited By

  • Silicon-carbon negative electrode material and preparation method therefor

    WO2026143476A1