Carbon nanocage loaded bimetallic sulfide as well as preparation method and application thereof

By using carbon nanocage-loaded bimetal sulfide ultra-thin two-dimensional nanosheets in sodium ion battery electrode materials, the problems of poor cycle stability and insufficient conductivity of bi-transition metal sulfide in sodium ion battery are solved, and the problem of poor circulation stability and insufficient conductivity of bi-transition metal sulfide in sodium ion battery is achieved. High electrochemical properties and lower preparation costs.

CN118970002AInactive Publication Date: 2024-11-15SHAANXI UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411043723.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When double transition metal sulfide is used as a sodium ion battery electrode material, there are problems such as poor cycle stability and low first-time Coulomb efficiency.

Method used

Using the preparation method of carbon nanocage-loaded bimetal sulfide, the carbon nanocage is combined with molybdenum salt, thiourea and carbon nanocage in hydrothermal reaction to form ultra-thin two-dimensional nanosheets of carbon nanocage-loaded bimetal sulfide, using carbon nanometers The rigidity and porous structure of the cage improve the physical support of the material and the ion diffusion channel, enhancing the efficiency of electrochemical reactions.

Benefits of technology

It improves the cyclic stability and conductivity of the material, reduces volume expansion and structural collapse during charging and discharging, speeds up electron transfer speed, improves electrochemical reaction efficiency, and reduces preparation costs, making it suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970002A_ABST
    Figure CN118970002A_ABST
Patent Text Reader

Abstract

The invention discloses a carbon nanocage loaded bimetallic sulfide as well as a preparation method and application thereof, and belongs to the technical field of transition metal sulfide composite materials. According to the preparation method disclosed by the invention, the rigid structure of the carbon nanocage can provide physical support for the metal sulfide, reduce volume expansion and structure collapse in the charge-discharge process and improve the cycling stability of the material, and the carbon material has good conductivity, so that when the metal sulfide is loaded on the carbon nanocage, the conductivity of the material is improved. The conductivity of the whole material can be further improved, so that the electron transmission speed is accelerated; the porous structure of the carbon nanocage and the nanosheet structure formed by vertically interweaving the bimetallic sulfides provide a rapid diffusion channel for ions. The method is simple in preparation process, low in cost and easy for large-scale production, and the prepared composite material is green in raw material and environment-friendly in preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of transition metal sulfide composite materials, and specifically relates to a carbon nano cage loaded bimetallic sulfide and a preparation method and application thereof. Background Art

[0002] Double transition metal sulfides are a class of compounds composed of two different transition metal elements and sulfur, with unique physical and chemical properties, such as complex electronic structure, good conductivity, higher thermal stability, chemical stability, nonlinear optical effects, etc. These compounds usually show better physical properties and chemical stability than single transition metal sulfides, which makes them widely used in energy storage, catalysis, optoelectronics such as photodetectors and solar cells, environmental protection such as wastewater treatment and exhaust gas purification, materials science such as alloys, wear-resistant materials and other fields.

[0003] Double transition metal sulfides have also shown great application potential in the field of sodium ion batteries due to their unique structure and properties. As electrode materials for sodium ion batteries, double transition metal sulfides have the following characteristics, such as high theoretical specific capacity, structural diversity, good chemical stability, optimized ion diffusion paths, etc. However, they also have the following disadvantages, such as the need to further improve conductivity, large volume expansion, which may lead to the destruction of the material structure, affect the cycle stability of the battery, and low first coulombic efficiency. Summary of the invention

[0004] The object of the present invention is to provide a carbon nanocage-loaded bimetallic sulfide and a preparation method and application thereof, so as to solve the technical problem that the existing bitransition metal sulfide has poor cycle stability when used as an electrode material for sodium ion batteries.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions: The present invention discloses a method for preparing a carbon nano cage-loaded bimetallic sulfide, comprising the following steps: After mixing molybdenum salt, thiourea and deionized water, carbon nanocages are added to obtain a mixed solution A; The mixed solution A is subjected to a hydrothermal reaction, and after the reaction is completed, the precipitate is collected, washed, and dried in sequence to obtain a carbon nanocage-loaded bimetallic sulfide.

[0006] Furthermore, the usage ratio of the molybdenum salt, thiourea, deionized water and carbon nanocage is 1 mmol: (3-5) mmol: (40-60) mL: (10-20) mg.

[0007] Furthermore, the molybdenum salt is one or more of ammonium molybdate, sodium molybdate and potassium molybdate.

[0008] Furthermore, the method for preparing the carbon nanocage comprises the following steps: After mixing and stirring the zinc salt, the complexing agent and anhydrous methanol, the product is collected, washed and dried in sequence to obtain a precursor; The precursor and dopamine are added into deionized water, the product is collected after stirring, and calcined in an inert atmosphere to obtain a carbon nanocage.

[0009] Furthermore, the dosage ratio of the zinc salt, the complexing agent and the anhydrous methanol is (1-3) g: (1-3) g: 150 mL; and the mixing and stirring time is 10-20 h.

[0010] Furthermore, in the step of calcining in an inert atmosphere to obtain carbon nanocages, the amount ratio of the precursor, dopamine and deionized water is 100 mg: (10-20) mg: 150 mL, the stirring time is 10-12 h; the calcination temperature is 700-900 ° C, and the time is 1-3 h; The zinc salt is one of zinc nitrate, zinc sulfate or zinc carbonate; the complexing agent is one of 4-hydroxymethylimidazole, 2-hydroxymethyl-1-methylimidazole or 2-chloromethylimidazole.

[0011] Furthermore, the temperature of the hydrothermal reaction is 180-210° C., the heating rate is 5° C. per minute, and the hydrothermal reaction time is 18-24 hours.

[0012] The invention also discloses carbon nano cage loaded bimetallic sulfide prepared by the preparation method.

[0013] Furthermore, the microstructure of the carbon nanocage-loaded bimetallic sulfide is composed of carbon nanocage-loaded bimetallic sulfide ultrathin two-dimensional nanosheets, and the thickness of the ultrathin two-dimensional nanosheets is 20 nm.

[0014] The invention also discloses the application of the carbon nano cage loaded bimetallic sulfide in the electrode material of sodium ion battery.

[0015] Compared with the prior art, the present invention has the following beneficial effects: The invention discloses a preparation method of carbon nano cage loaded bimetallic sulfide. Molybdenum salt, thiourea and carbon nano cage are used as raw materials. A complexing agent is introduced and the components and nanostructure of the composite material are reasonably adjusted. The rigid structure of the carbon nano cage can provide physical support for the metal sulfide, reduce volume expansion and structural collapse during charge and discharge, and improve the cycle stability of the material. The carbon material itself has good electrical conductivity. When the metal sulfide is loaded on the carbon nano cage, the electrical conductivity of the overall material can be further improved, thereby accelerating the electron transmission speed. The porous structure of the carbon nano cage and the vertically interwoven nanosheet structure of the bimetallic sulfide not only provide a channel for rapid diffusion of ions, but also help to increase the number of active sites and improve the electrochemical reaction efficiency of the composite material.

[0016] Furthermore, the method has a simple preparation process, low cost, and is easy for large-scale production. The prepared composite material has green raw materials and an environmentally friendly preparation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a SEM image of the carbon nanocage loaded with bimetallic sulfide prepared by the present invention; Figure 2 This is a TEM image of the carbon nanocage loaded with bimetallic sulfide prepared by the present invention; Figure 3 This is the XRD pattern of the carbon nanocage loaded bimetallic sulfide prepared by the present invention; Figure 4 This is a charge and discharge curve diagram of the carbon nanocage loaded with bimetallic sulfide prepared by the present invention. DETAILED DESCRIPTION

[0018] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.

[0019] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0020] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0021] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”

[0022] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0023] The present invention provides a method for preparing a carbon nanocage-supported bimetallic sulfide, comprising the following steps: S1: 1 mmol of molybdenum salt and 3-5 mmol of thiourea were ultrasonically dissolved in 40-60 mL of deionized water, and then a certain amount of carbon nanocages were ultrasonically dispersed to prepare a mixed solution A; S2: placing the mixed solution A in a stainless steel reactor for hydrothermal reaction, collecting the precipitate after the reaction, washing it, and drying it to prepare carbon nanocage-loaded bimetallic sulfide.

[0024] Preferably, in S1, the molybdenum salt includes but is not limited to ammonium molybdate, sodium molybdate, and potassium molybdate.

[0025] Preferably, in S1, the dispersed amount of the carbon nanocage is 10-20 mg. The steps for preparing the carbon nanocage are as follows: The zinc salt (1-3 g) and the complexing agent (1-3 g) were ultrasonically dissolved in 150 mL of anhydrous methanol, stirred at room temperature for 10-20 h, and the product was collected, washed, and dried to prepare a precursor; The zinc salt includes but is not limited to zinc nitrate, zinc sulfate, zinc carbonate, and the complexing agent includes but is not limited to 4-hydroxymethylimidazole, 2-hydroxymethyl-1-methylimidazole, and 2-chloromethylimidazole; 100 mg of the above precursor and 10-20 mg of dopamine were added to 150 mL of deionized water, stirred at room temperature for 10-12 h, the product was collected, and calcined at 700-900° C. in an argon atmosphere for 1-3 h to prepare a carbon nanocage.

[0026] Preferably, in S2, the thermal reaction temperature is 180-210°C, the heating rate is 5°C per minute, and the hydrothermal reaction time is 18-24h.

[0027] The invention also discloses carbon nano cage loaded bimetallic sulfide prepared by the preparation method.

[0028] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0029] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.

[0030] Example 1 A method for preparing a carbon nanocage-supported bimetallic sulfide comprises the following steps: S1: 1 mmol potassium molybdate (molybdenum salt) and 5 mmol thiourea were ultrasonically dissolved in 60 mL of deionized water, and then 20 mg of carbon nanocages were ultrasonically dispersed to obtain a mixed solution A; The steps for preparing the carbon nanocage are as follows: 3 g of zinc nitrate (zinc salt) and 3 g of 4-hydroxymethylimidazole (complexing agent) were ultrasonically dissolved in 150 mL of anhydrous methanol, stirred at room temperature for 20 h, and the product was collected, washed, and dried to prepare a precursor; 100 mg of the above precursor and 20 mg of dopamine were added to 150 mL of deionized water, stirred at room temperature for 12 h, the product was collected, and calcined at 900° C. for 3 h in an argon atmosphere to obtain the carbon nanocage; S2: The mixed solution A is placed in a stainless steel reactor for hydrothermal reaction. The hydrothermal reaction temperature is 210°C, the heating rate is 5°C per minute, and the hydrothermal reaction time is 24 hours. After the reaction, the precipitate is collected, washed, and dried to obtain carbon nanocage-loaded bimetallic sulfide.

[0031] Example 2 A method for preparing a carbon nanocage-supported bimetallic sulfide comprises the following steps: S1: 1 mmol sodium molybdate (molybdenum salt) and 50 mmol thiourea were ultrasonically dissolved in 50 mL of deionized water, and then 15 mg of carbon nanocages were ultrasonically dispersed to obtain a mixed solution A; The steps for preparing the carbon nanocage are as follows: 2 g of zinc sulfate (zinc salt) and 2 g of 2-hydroxymethyl-1-methylimidazole (complexing agent) were ultrasonically dissolved in 150 mL of anhydrous methanol, stirred at room temperature for 15 h, and the product was collected, washed, and dried to prepare a precursor; 100 mg of the above precursor and 15 mg of dopamine were added to 150 mL of deionized water, stirred at room temperature for 10 h, the product was collected, and calcined at 750° C. for 2 h in an argon atmosphere to obtain the carbon nanocage; S2: Place the mixed solution A in a stainless steel reactor for hydrothermal reaction. The hydrothermal reaction temperature is 200°C, the heating rate is 5°C per minute, and the hydrothermal reaction time is 20 hours. After the reaction, collect the precipitate, wash it, and dry it to obtain carbon nanocage-loaded bimetallic sulfide.

[0032] Example 3 A method for preparing a carbon nanocage-supported bimetallic sulfide comprises the following steps: S1: 1 mmol potassium molybdate (molybdenum salt) and 3 mmol thiourea were ultrasonically dissolved in 40 mL of deionized water, and then 10 mg of carbon nanocages were ultrasonically dispersed to obtain a mixed solution A; The steps for preparing the carbon nanocage are as follows: 1 g of zinc carbonate (zinc salt) and 1 g of 2-chloromethylimidazole (complexing agent) were ultrasonically dissolved in 150 mL of anhydrous methanol, stirred at room temperature for 10 h, and the product was collected, washed, and dried to prepare a precursor; 100 mg of the above precursor and 10 mg of dopamine were added to 150 mL of deionized water, stirred at room temperature for 10 h, the product was collected, and calcined at 700° C. in an argon atmosphere for 1 h to obtain the carbon nanocage; S2: Place the mixed solution A in a stainless steel reactor for hydrothermal reaction. The hydrothermal reaction temperature is 180°C, the heating rate is 5°C per minute, and the hydrothermal reaction time is 18 hours. After the reaction, collect the precipitate, wash it, and dry it to obtain carbon nanocage-loaded bimetallic sulfide.

[0033] Example 4 A method for preparing a carbon nanocage-supported bimetallic sulfide comprises the following steps: S1: 1 mmol of sodium molybdate (molybdenum salt) and 3 mmol of thiourea were ultrasonically dissolved in 55 mL of deionized water, and then 15 mg of carbon nanocages were ultrasonically dispersed to obtain a mixed solution A; The steps for preparing the carbon nanocage are as follows: 2 g of zinc sulfate (zinc salt) and 1 g of 2-chloromethylimidazole (complexing agent) were ultrasonically dissolved in 150 mL of anhydrous methanol, stirred at room temperature for 10 h, and the product was collected, washed, and dried to prepare a precursor; 100 mg of the above precursor and 15 mg of dopamine were added to 150 mL of deionized water, stirred at room temperature for 10 h, the product was collected, and calcined at 800° C. for 2 h in an argon atmosphere to obtain the carbon nanocage; S2: Place the mixed solution A in a stainless steel reactor for hydrothermal reaction. The hydrothermal reaction temperature is 200°C, the heating rate is 5°C per minute, and the hydrothermal reaction time is 20 hours. After the reaction, collect the precipitate, wash it, and dry it to obtain carbon nanocage-loaded bimetallic sulfide.

[0034] Example 5 A method for preparing a carbon nanocage-supported bimetallic sulfide comprises the following steps: S1: 1 mmol potassium molybdate (molybdenum salt) and 4 mmol thiourea were ultrasonically dissolved in 60 mL of deionized water, and then 20 mg of carbon nanocages were ultrasonically dispersed to obtain a mixed solution A; The steps for preparing the carbon nanocage are as follows: 3 g of zinc nitrate (zinc salt) and 2 g of 2-chloromethylimidazole (complexing agent) were ultrasonically dissolved in 150 mL of anhydrous methanol, stirred at room temperature for 20 h, and the product was collected, washed, and dried to prepare a precursor; 100 mg of the above precursor and 20 mg of dopamine were added to 150 mL of deionized water, stirred at room temperature for 12 h, the product was collected, and calcined at 850° C. in an argon atmosphere for 3 h to obtain the carbon nanocage; S2: The mixed solution A is placed in a stainless steel reactor for hydrothermal reaction. The hydrothermal reaction temperature is 210°C, the heating rate is 5°C per minute, and the hydrothermal reaction time is 18 hours. After the reaction, the precipitate is collected, washed, and dried to obtain carbon nanocage-loaded bimetallic sulfide.

[0035] Figure 1 This is a SEM image of the carbon nanocage-loaded bimetallic sulfide prepared in the present invention. From the image, it can be seen that the microstructure of the carbon nanocage-loaded bimetallic sulfide is composed of ultra-thin two-dimensional nanosheets of carbon nanocage-loaded bimetallic sulfide, and the thickness of the ultra-thin two-dimensional nanosheet is 20 nm.

[0036] Figure 2 This is a TEM image of the carbon nanocage loaded with bimetallic sulfide prepared in the present invention. It can be seen that the carbon nanocage is about 150 nm in size and about 30 nm in wall thickness.

[0037] Figure 3 This is the XRD diagram of the carbon nanocage loaded with bimetallic sulfide prepared by the present invention. From the figure, it can be seen that the product is composed of MoS2, ZnS, and C.

[0038] Figure 4This is a charge and discharge curve diagram of the carbon nanocage-loaded bimetallic sulfide prepared by the present invention. From the diagram, it can be seen that the prepared composite electrode material has a first discharge specific capacity of 600mAh / g at 0.1A / g, a first coulombic efficiency of 78%, and a discharge specific capacity of 400mAh / g after 100 cycles.

[0039] Table 1 is a comparison of the electrochemical properties of the product prepared by the present invention and the comparative example. It can be seen from the table that after the bimetallic sulfide is composited with the carbon nanocage, its comprehensive electrochemical properties such as specific capacity, first coulombic efficiency, and cycle stability are all improved.

[0040] Table 1 Comparison of electrochemical performance of the products prepared by the present invention and the control samples

[0041] The above contents are only for explaining the technical idea of ​​the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing carbon nanocage-supported bimetallic sulfide, characterized in that: The following steps are involved: After mixing molybdenum salt, thiourea and deionized water, carbon nanocages are added to obtain a mixed solution A; The mixed solution A is subjected to a hydrothermal reaction, and after the reaction is completed, the precipitate is collected, washed, and dried in sequence to obtain a carbon nanocage-loaded bimetallic sulfide.

2. The method for preparing a carbon nanocage-supported bimetallic sulfide according to claim 1, characterized in that: The usage ratio of the molybdenum salt, thiourea, deionized water and carbon nano cage is 1 mmol: (3-5) mmol: (40-60) mL: (10-20) mg.

3. The method for preparing a carbon nanocage-supported bimetallic sulfide according to claim 1, characterized in that: The molybdenum salt is one or more of ammonium molybdate, sodium molybdate and potassium molybdate.

4. The method for preparing a carbon nanocage-supported bimetallic sulfide according to claim 1, characterized in that: The method for preparing the carbon nano cage comprises the following steps: After mixing and stirring the zinc salt, the complexing agent and anhydrous methanol, the product is collected, washed and dried in sequence to obtain a precursor; The precursor and dopamine are added into deionized water, the product is collected after stirring, and calcined in an inert atmosphere to obtain a carbon nanocage.

5. The method for preparing a carbon nanocage-supported bimetallic sulfide according to claim 4, characterized in that: In the step of preparing the precursor, the usage ratio of the zinc salt, the complexing agent and the anhydrous methanol is (1-3) g: (1-3) g: 150 mL; and the mixing and stirring time is 10-20 hours.

6. The method for preparing a carbon nanocage-supported bimetallic sulfide according to claim 4, characterized in that: In the step of calcining in an inert atmosphere to obtain carbon nanocages, the ratio of the precursor, dopamine and deionized water is 100 mg: (10-20) mg: 150 mL, the stirring time is 10-12 hours, the calcination temperature is 700-900° C., and the time is 1-3 hours; The zinc salt is one of zinc nitrate, zinc sulfate or zinc carbonate; the complexing agent is one of 4-hydroxymethylimidazole, 2-hydroxymethyl-1-methylimidazole or 2-chloromethylimidazole.

7. The method for preparing a carbon nanocage-supported bimetallic sulfide according to claim 1, characterized in that: The temperature of the hydrothermal reaction is 180-210° C., the heating rate is 5° C. per minute, and the hydrothermal reaction time is 18-24 hours.

8. A carbon nanocage loaded with bimetallic sulfide, characterized in that: The preparation method is described in any one of claims 1 to 7.

9. The carbon nanocage-supported bimetallic sulfide according to claim 8, characterized in that: The microstructure of the carbon nanocage-supported bimetallic sulfide is composed of an ultra-thin two-dimensional nanosheet of carbon nanocage-supported bimetallic sulfide, and the thickness of the ultra-thin two-dimensional nanosheet is 20 nm.

10. Use of the carbon nanocage-loaded bimetallic sulfide according to claim 8 or 9 in a sodium ion battery electrode material.