Hydrogel electrolyte, preparation method thereof and thermal battery

By stretching and immersing the hydrogel, its network structure is optimized, and the problem that hydrogel electrolyte is difficult to meet the thermoelectrochemical and mechanical properties at the same time is improved, and its applicability in flexible and wearable electronic devices is improved. and performance.

CN118970221APending Publication Date: 2024-11-15SHENZHEN UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411011600.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The thermoelectrochemical and mechanical properties of existing hydrogel electrolytes are difficult to meet at the same time, especially in flexible and wearable electronic devices, where electrolyte leakage and complex packaging problems exist.

Method used

The network structure of the hydrogel is optimized and enhanced by stretching the hydrogel in a mixture of 2-methacryloyloxyethylphosphorylcholine and inorganic redox pairs Mechanical strength and thermoelectric properties.

Benefits of technology

The mechanical strength and thermoelectrochemical properties of hydrogel electrolytes are improved, making them more suitable for applications in flexible and wearable electronic devices, reducing the risk of electrolyte leakage, and improving the output power and mechanical properties of thermal batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970221A_ABST
    Figure CN118970221A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electronic science, and discloses a hydrogel electrolyte and a preparation method thereof, and a thermal battery, the preparation method of the hydrogel electrolyte comprises the following steps: stretching hydrogel in a predetermined direction; the stretched hydrogel is soaked in a mixed solution containing 2-methacryloyloxyethyl phosphorylcholine and an inorganic redox couple for a preset time, and the hydrogel electrolyte is obtained. According to the invention, a directional pre-stretching method is adopted, redox ion pairs and zwitterions are introduced, and the hydrogel electrolyte is synergistically regulated on the aspects of thermoelectric chemical properties and mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electronic information technology, and in particular to a hydrogel electrolyte and a preparation method thereof, and a thermal battery. Background Art

[0002] The rapid development of wearable electronics has triggered an urgent need for efficient energy supply systems. Compared with traditional energy technologies such as supercapacitors, lithium-ion batteries, and solar cells, thermoelectric conversion devices have the advantages of no noise, zero emissions, and low maintenance requirements. In terms of the collection and application of low-grade thermal energy (≤170°C), they provide an attractive energy supply solution for the development of flexible and wearable electronics. In the past few decades, traditional solid thermoelectric materials have been well studied, but their mechanical rigidity, toxicity, high cost, and relatively low thermoelectrochemical Seebeck coefficient (S) at room temperature have limited their application prospects. e ) hinders its further development in flexible and wearable applications. In contrast, thermal batteries (TECs) have high S e TECs can effectively convert low-grade thermal energy into electrical energy, which has attracted widespread attention in recent years. Hydrogel-type TECs can effectively avoid the risk of electrolyte leakage by introducing a cross-linked network structure to restrict the free flow of water molecules, so that they can be better applied to many fields such as flexible and wearable electronics, and are expected to solve the electrolyte leakage and complex packaging problems existing in traditional solution-type TECs.

[0003] In recent years, hydrogel-based TECs have made some progress in the structural design of electrolytes, preparation methods and processes, internal carrier transport mechanisms, the effects of ion types and concentrations on thermoelectrochemical properties, and accurate measurements of hydrogel thermoelectrochemical properties, and have rapidly developed into a hot topic in the field of flexible and wearable electronics. However, compared with solution-based TECs, there is still a large gap in the depth and breadth of research on hydrogel-based TECs. Current research is still in its infancy, focusing more on the realization of electrolyte gelation of hydrogel-based TECs and the design of flexible wearable devices, while there is still a lack of systematic research on the thermoelectrochemical mechanism and influence rules in the gel matrix. For the existing hydrogel electrolytes, it is difficult to meet both thermoelectrochemical and mechanical properties in many cases.

[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the present invention provides a hydrogel electrolyte and a preparation method thereof, and a thermal battery, so as to solve the problem that the thermoelectrochemical properties and mechanical properties of the existing hydrogel electrolytes are difficult to meet simultaneously in many cases.

[0006] The technical solution adopted by the present invention to solve the above technical problems is as follows:

[0007] In a first aspect of the present invention, a method for preparing a hydrogel electrolyte is provided, the preparation method comprising the following steps:

[0008] stretching the hydrogel in a predetermined direction;

[0009] The stretched hydrogel is immersed in a mixed solution containing 2-methacryloyloxyethyl phosphorylcholine and an inorganic redox pair for a predetermined time to obtain the hydrogel electrolyte.

[0010] Preferably, the inorganic redox pair is selected from Fe(CN)6 3- / Fe(CN)6 4- 、SO4 2- / SO3 2- , Fe 2+ / Fe 3+ A pair in .

[0011] Preferably, in the mixed solution, the molar concentration of 2-methacryloyloxyethyl phosphorylcholine is 0.5M-3M.

[0012] Preferably, in the mixed solution, the molar concentration of the inorganic redox pair is 0.05M-0.4M.

[0013] Preferably, the hydrogel is selected from one of PVA hydrogel, gelatin hydrogel and cellulose hydrogel.

[0014] Preferably, the stretched hydrogel is immersed in the mixed solution for a predetermined immersion time of 6-48 hours.

[0015] Preferably, the stretching ratio of the stretching is 0-150%.

[0016] Preferably, the stretching is maintained for 6-48 hours.

[0017] A second aspect of the present invention provides a hydrogel electrolyte, which is prepared by the above-mentioned preparation method.

[0018] According to a second aspect of the present invention, a thermal battery is provided. The thermal battery comprises a hydrogel electrolyte and electrodes assembled on both sides of the hydrogel electrolyte. The hydrogel electrolyte adopts the above-mentioned hydrogel electrolyte.

[0019] Beneficial effects:

[0020] The invention discloses a hydrogel electrolyte and a preparation method thereof, and a thermal battery. The invention first stretches the hydrogel in a predetermined direction, which can change the internal network structure of the hydrogel material, thereby improving its mechanical strength and toughness, so that it is not easy to break when subjected to external force. Then the stretched hydrogel is immersed in a mixed solution containing 2-methacryloyloxyethyl phosphorylcholine and an inorganic redox pair, wherein 2-methacryloyloxyethyl phosphorylcholine is a zwitterion, and its abundant choline cation and phosphate anion groups can enter the interconnected hydrogel network, and the hydrogel chain is tightly bound through non-covalent interactions (including hydrogen bonds and electrostatic interactions); at the same time, as an anion in the Hofmeister sequence, it can optimize the network structure in the hydrogel through the salting-out effect, enhance chain aggregation, and improve the mechanical strength of the hydrogel electrolyte; in addition, there is a stronger interaction between 2-methacryloyloxyethyl phosphorylcholine and the redox ion pair, so that its thermoelectrochemical performance is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 (a) is the anion sequence in the Hofmeister effect; (b) is the "salting out" and "salting in" effects in the Hofmeister effect.

[0022] Figure 2 This is a picture and schematic diagram of the structure of the hydrogel after directional stretching in Example 1 of the present invention;

[0023] Figure 3 Graphs showing stretching curves of the hydrogels in Examples 1-4 of the present invention at different stretching ratios;

[0024] Figure 4 The power output of the hydrogels in Examples 1-4 of the present invention when stretched at different ratios;

[0025] Figure 5 This is a functional relationship diagram of the temperature difference and voltage of the hydrogel electrolyte prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0026] The present invention provides a hydrogel electrolyte and a preparation method thereof, and a thermal battery. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0027] An embodiment of the present invention provides a method for preparing a hydrogel electrolyte, the preparation method comprising the following steps:

[0028] stretching the hydrogel in a predetermined direction;

[0029] The stretched hydrogel is immersed in a mixed solution containing 2-methacryloyloxyethyl phosphorylcholine and an inorganic redox pair for a predetermined time to obtain the hydrogel electrolyte.

[0030] The embodiment of the present invention first stretches the hydrogel in a predetermined direction. On the one hand, stretching in a predetermined direction can change the internal network structure of the hydrogel material, thereby improving its mechanical strength and toughness, making it less likely to break when subjected to external force. On the other hand, considering the randomness of the spontaneous polymerization of the hydrogel, the porous network structure of the polymer is isotropic and disordered, which enhances the resistance to internal migration, thereby affecting the transport mechanics. The embodiment of the present invention establishes an ion transport channel by directional stretching to induce the orientation of the arranged polymer chains, thereby optimizing the ion transport resistance and enhancing its output performance.

[0031] The stretched hydrogel is then immersed in a mixed solution containing 2-methacryloyloxyethyl phosphorylcholine and an inorganic redox pair. 2-methacryloyloxyethyl phosphorylcholine, as a zwitterion (its molecular structure is shown in the figure below), can kill two birds with one stone and synergistically regulate the thermoelectrochemical and mechanical properties of the hydrogel electrolyte. Specifically, as a Hofmeister sequence ion, this ion pair can optimize the network structure inside the hydrogel through the salting-out effect, enhance chain aggregation, and improve the mechanical strength of the hydrogel electrolyte. Among them, the Hofmeister effect significantly improves the mechanical properties, fatigue resistance and energy dissipation capacity of the hydrogel by changing the interaction and hydration of the polymer chains in the hydrogel. Such as Figure 1 As shown in the figure, the salt ions in the middle of the Hofmeister sequence have little effect on the solubility of the hydrophilic polymer in aqueous solution. However, the salt ions on the left side of the Hofmeister sequence will produce a salting-out effect, forming hydrogen bonds between the hydroxyl groups of the polymer chains, leading to the aggregation / crystallization of the polymer chains; while the salt ions on the right side of the Hofmeister sequence will produce a salting-in effect, breaking the hydrogen bonds between the hydrogel chains caused by the ions, causing the chains to relax. In addition, the choline cations and phosphate anion groups in the 2-methacryloyloxyethyl phosphorylcholine molecules enter the interconnected hydrogel network, tightly connecting the hydrogel chains through non-covalent interactions (including hydrogen bonds and electrostatic interactions), further improving the mechanical properties of the hydrogel. There is a stronger interaction between 2-methacryloyloxyethyl phosphorylcholine and the redox ion pairs, which expands the entropy difference of the redox reaction and improves the thermoelectrochemical performance.

[0032]

[0033] In some embodiments, the inorganic redox pair is selected from Fe(CN)6 3- / Fe(CN)6 4- 、SO4 2- / SO32- , Fe 2+ / Fe 3+ A pair in .

[0034] In some embodiments, in the mixed solution, the molar concentration of 2-methacryloyloxyethyl phosphorylcholine is 0.5M-3M. The molar concentration of 2-methacryloyloxyethyl phosphorylcholine may be 0.5M, 1M, 1.5M, 2M, 2.5M, or 3M.

[0035] When the concentration of 2-methacryloyloxyethyl phosphorylcholine is low, it has little effect on the solvation shell of the inorganic redox ion pair, the entropy difference of the inorganic redox ion pair is not increased, the Seebeck coefficient is slightly increased, and the mechanical properties of the hydrogel electrolyte are not improved much. When the concentration is too high, it will increase the overall viscosity of the electrolyte, hinder ion migration, and reduce the Seebeck coefficient.

[0036] In some preferred embodiments, in the mixed solution, the molar concentration of 2-methacryloyloxyethyl phosphorylcholine is 2.5M.

[0037] In some embodiments, in the mixed solution, the molar concentration of the inorganic redox pair is 0.05 M-0.4 M. The molar concentration of the inorganic redox pair may be 0.05, 0.1 M, 0.2 M, 0.3 M, or 0.4 M.

[0038] When the concentration of inorganic redox ion pairs is too low, the number of ion migration is small, the transfer charge is insufficient, and a high thermoelectric potential cannot be provided. When the concentration of inorganic redox ion pairs is too high, the solution becomes viscous, the ion migration is hindered, the transfer charge is reduced, and the thermoelectric potential cannot achieve a good effect.

[0039] In some preferred embodiments, in the mixed solution, the molar concentration of the inorganic redox pair is 0.2M.

[0040] In some embodiments, the hydrogel is selected from one of PVA hydrogel, gelatin hydrogel, and cellulose hydrogel.

[0041] In some embodiments, a method for preparing a PVA hydrogel is provided, the preparation method comprising the following steps:

[0042] One-pot method for preparing PVA hydrogel: using deionized water as solvent, adding 15 wt% PVA into a 100 mL beaker, heating and stirring at 95 °C for 1 hour to form a stable precursor solution;

[0043] The precursor solution was poured into a glass plate mold and cooled at room temperature to form the product, and then freeze-thawed for 3 times at -20°C, with each cycle lasting 24 hours;

[0044] The PVA hydrogel after freeze-thaw cycles was cut into rectangles of specified size, 10 mm × 30 mm.

[0045] In some embodiments, the mass concentration of the PVA is 5%-20%, preferably 15%.

[0046] In some embodiments, the stretched hydrogel is immersed in the mixed solution for a predetermined immersion time of 6-48 hours.

[0047] In some preferred embodiments, the stretched hydrogel is immersed in the mixed solution for a predetermined immersion time of 24 hours.

[0048] In some embodiments, the stretching ratio of the stretching is 0-150%. The stretching ratio of the stretching can be 0%, 25%, 50%, 75%, 100%, or 150%.

[0049] The formula for the stretching rate is: (L2-L1) / L1×100%. Among them, L1 is the length of the material before stress, and L2 is the length of the material after stress. When the stretching rate is too small, its internal network structure is random and disordered, and the mechanical properties of the hydrogel electrolyte are poor. The appropriate stretching rate provides a way to decouple mechanical properties and output power through a hierarchical structure. The oriented and partially crystallized fibrils increase the toughness and fatigue threshold, and ions can be quickly transported along the nanochannels of the fibers. However, excessive stretching rates will damage the physical cross-linking network of the hydrogel electrolyte, resulting in a decrease in the final mechanical properties.

[0050] In some preferred embodiments, the stretching ratio of the stretching is 150%.

[0051] In some embodiments, the stretching is maintained for 6-48 hours.

[0052] In some preferred embodiments, the stretching is maintained for 24 hours.

[0053] The embodiment of the present invention further provides a hydrogel electrolyte, which is prepared by the above-mentioned preparation method.

[0054] An embodiment of the present invention further provides a thermal battery, which includes a hydrogel electrolyte and electrodes assembled on both sides of the hydrogel electrolyte, wherein the hydrogel electrolyte adopts the above-mentioned hydrogel electrolyte.

[0055] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, and are only for illustrating the present invention but not limiting the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.

[0056] Example 1

[0057] A preparation of a thermal battery comprises the following steps:

[0058] Preparation of hydrogel electrolyte:

[0059] (1) Preparation of PVA hydrogel by one-pot method: Using deionized water as solvent, add PVA with a mass concentration of 15 wt% into a 100 mL beaker, heat and stir at 95°C for 1 hour to form a stable precursor solution; pour the precursor solution into a glass plate mold and cool it at room temperature to form it, and freeze-thaw cycle it at -20°C for 3 times, each cycle lasting 24 hours; cut the PVA hydrogel after freeze-thaw cycle into a rectangle of specified size, with a size of 10 mm × 30 mm.

[0060] (2) The PVA hydrogel of step (1) was pre-stretched in a directional manner, and pre-stretched by 150% in the horizontal direction, and the PVA hydrogel was packaged with a polyimide tape, and the stretching time was maintained for 24 hours. Figure 2 .

[0061] (3) A mixed solution of 2.5 M 2-methacryloyloxyethyl phosphorylcholine, 0.2 M K3[Fe(CN)6] and K4[Fe(CN)6] was prepared at room temperature. The pre-stretched PVA hydrogel was immersed in the solution for 24 h to obtain a hydrogel electrolyte.

[0062] Preparation of thermal battery: The prepared hydrogel electrolyte, flexible carbon-based electrode and aqueous polyurethane packaging material are packaged to complete the preparation of the thermal battery.

[0063] The conductivity of the obtained hydrogel electrolyte is 2.5 S m -1 , Seebeck coefficient is 2.8mV K -1 The obtained thermal battery has a maximum output power density of 1059.9 μW m at a temperature difference of 30 K. 2 , the tensile strength is 21.4Mpa.

[0064] Example 2

[0065] Preparation of a thermal battery. The preparation method of this embodiment is basically the same as that of Example 1, except that in step (2) of preparing the hydrogel electrolyte, 100% pre-stretching is performed in the horizontal direction.

[0066] The conductivity of the obtained hydrogel electrolyte is 1.24 S m -1 , Seebeck coefficient is 2.79mV K -1 The obtained thermal battery has a maximum output power of 526.2 μW m at a temperature difference of 30 K. 2 , the tensile strength is 16.33Mpa.

[0067] Example 3

[0068] Preparation of a thermal battery. The preparation method of this embodiment is basically the same as that of embodiment 1, except that in step (2) of preparing the hydrogel electrolyte, 50% pre-stretching is performed in the horizontal direction.

[0069] The conductivity of the obtained hydrogel electrolyte is 1.15 S m -1 , Seebeck coefficient is 2.81mV K -1 The obtained thermal battery has a maximum output power of 434.2 μW m at a temperature difference of 30 K. 2 , the tensile strength is 12.87Mpa.

[0070] Example 4

[0071] Preparation of a thermal battery. The preparation method of this embodiment is basically the same as that of Example 1, except that in step (2) of preparing the hydrogel electrolyte, 0% pre-stretching is performed in the horizontal direction.

[0072] The conductivity of the obtained hydrogel electrolyte is 0.8 S m -1 , Seebeck coefficient is 2.8mV K -1 The obtained thermal battery has a maximum output power of 277.7 μW m at a temperature difference of 30 K. 2 , the tensile strength is 5.65Mpa.

[0073] Example 5

[0074] Preparation of a thermal battery. The preparation method of this embodiment is basically the same as that of Example 1, except that in step (3) of preparing the hydrogel electrolyte, the prepared mixed solution does not contain 2-methacryloyloxyethyl phosphorylcholine.

[0075] The conductivity of the obtained hydrogel electrolyte is 0.5 S m -1 , Seebeck coefficient is 1.47mV K -1The obtained thermal battery has a maximum output power of 319.8 μW m at a temperature difference of 30 K. 2 , the tensile strength is 0.51Mpa.

[0076] Example 6

[0077] Preparation of a thermal battery. The preparation method of this embodiment is basically the same as that of Example 1, except that in step (3) of preparing the hydrogel electrolyte, the K3[Fe(CN)6] and K4[Fe(CN)6] in the prepared mixed solution are 0.1M.

[0078] The conductivity of the obtained hydrogel electrolyte is 1.14 S m -1 , Seebeck coefficient is 1.61mV K -1 The obtained thermal battery has a maximum output power of 521.1 μW m at a temperature difference of 30 K. 2 , the tensile strength is 20.3Mpa.

[0079] Comparative Example 1

[0080] Preparation of a thermal battery. The preparation method of this comparative example is basically the same as that of Example 1, except that in step (5) of preparing the hydrogel electrolyte, 2-methacryloyloxyethyl phosphorylcholine is replaced by betaine.

[0081] The conductivity of the obtained hydrogel electrolyte is 3.6 S m -1 , Seebeck coefficient is 1.65mV K -1 The obtained thermal battery has a maximum output power of 233.2 μW m at a temperature difference of 30 K. 2 , the tensile strength is 0.8Mpa.

[0082] Comparative Example 2

[0083] Preparation of a thermal battery. The preparation method of this comparative example is basically the same as that of Example 1, except that the PVA hydrogel prepared in step (1) is directly immersed in electrolyte for the preparation of the thermal battery, without the subsequent steps (2) and (3).

[0084] The conductivity of the obtained hydrogel electrolyte is 0.08 S m -1 , Seebeck coefficient is 1.41mV K -1 The obtained thermal battery has a maximum output power of 128.6 μW m at a temperature difference of 30 K. 2 , the tensile strength is 0.21Mpa. Among them, the Seebeck coefficient S e The formula is as follows:

[0085]

[0086] Where ΔV is the open circuit voltage, ΔT is the temperature difference, n is the number of electrons transferred in the redox reaction, F is the Faraday constant, and ΔS is the partial molar entropy difference of the redox pair.

[0087] Compared with betaine, 2-methacryloyloxyethyl phosphorylcholine makes the solvation shell of the inorganic redox pair more disordered, thereby making the molar entropy difference between the hot and cold ends of the thermal battery larger, the Seebeck coefficient higher, and the output power better; at the same time, the choline cation and phosphate anion groups of 2-methacryloyloxyethyl phosphorylcholine are more tightly bound to the PVA chain, further to the left in the Hofmeister sequence, and the salting-out effect is more obvious, which greatly improves the mechanical properties.

[0088] Figure 3 The stretching curves of the hydrogels in Examples 1-4 of the present invention at different stretching ratios are shown in the figure. It can be seen from the figure that when the stretching ratio is 150%, the mechanical properties of the hydrogels are the strongest.

[0089] Figure 4 The power output of the hydrogels in Examples 1-4 of the present invention at different stretching ratios is shown in the figure. It can be seen from the figure that the output power is the highest when the stretching ratio is 150%.

[0090] Figure 5 This is a functional relationship diagram of the temperature difference and voltage of the hydrogel electrolyte prepared in Example 1 of the present invention.

Claims

1. A method for preparing a hydrogel electrolyte, characterized in that: The preparation method comprises the following steps: stretching the hydrogel in a predetermined direction; The stretched hydrogel is immersed in a mixed solution containing 2-methacryloyloxyethyl phosphorylcholine and an inorganic redox pair for a predetermined time to obtain the hydrogel electrolyte.

2. The method for preparing a hydrogel electrolyte according to claim 1, characterized in that: The inorganic redox pair is selected from Fe(CN)6 3- / Fe(CN)6 4- 、SO4 2- / SO3 2- , Fe 2+ / Fe 3+ A pair in .

3. The method for preparing a hydrogel electrolyte according to claim 1, characterized in that: In the mixed solution, the molar concentration of 2-methacryloyloxyethyl phosphorylcholine is 0.5M-3M.

4. The method for preparing a hydrogel electrolyte according to claim 1, characterized in that: In the mixed solution, the molar concentration of the inorganic redox pair is 0.05M-0.4M.

5. The method for preparing a hydrogel electrolyte according to claim 1, characterized in that: The hydrogel is selected from one of PVA hydrogel, gelatin hydrogel and cellulose hydrogel.

6. The method for preparing a hydrogel electrolyte according to claim 1, characterized in that: The stretched hydrogel is immersed in the mixed solution for a predetermined immersion time of 6-48 hours.

7. The method for preparing a hydrogel electrolyte according to claim 1, characterized in that: The stretching ratio of the stretching is 0-150%.

8. The method for preparing a hydrogel electrolyte according to claim 1, characterized in that: The stretching is maintained for 6-48 hours.

9. A hydrogel electrolyte, characterized in that: The hydrogel electrolyte is prepared by the preparation method according to any one of claims 1 to 8.

10. A thermal battery, comprising a hydrogel electrolyte and electrodes assembled on both sides of the hydrogel electrolyte, characterized in that: The hydrogel electrolyte is the hydrogel electrolyte according to claim 9.

Citation Information

Cited By

  • Preparation method and application of ternary thermoelectric gel electrolyte based on bacterial nanocellulose

    CN119852557A

  • Waterborne polyurethane gel electrolyte, preparation method thereof and zinc ion battery

    CN119890483A