Composite lithium supplementing material and preparation method and application thereof
By using composite lithium supplement material in lithium-ion batteries, the combination of carbon cores and catalysts solves the problems of poor conductivity and high decomposition voltage, and improves the circulation efficiency and energy density of lithium-ion batteries, which are suitable for energy storage and New energy vehicles and other fields.
Patent Information
- Application Number
- CN202411016815.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
The poor conductivity and high decomposition voltage of lithium-ion batteries in existing lithium-ion batteries lead to low first-time cycle efficiency and reduced energy density of lithium-ion batteries, limiting their wide application in energy storage and new energy vehicles.
Using composite lithium supplement materials, including carbon cores, catalysts and lithium-rich materials, is prepared by hydrothermal reaction and calcination treatment. The catalyst is distributed around the carbon cores, and the lithium-rich materials are distributed around the catalyst to improve conductivity and reduce the decomposition voltage, thereby achieving Efficient lithium supplementation.
It improves the first cycle efficiency and reversible capacity of lithium-ion batteries, enhances electrochemical performance, and achieves high energy density and stability of cycling performance. It is suitable for energy storage and new energy vehicles.
Smart Images

Figure CN118970224A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of lithium battery technology, and in particular relates to a composite lithium supplement material and a preparation method and application thereof. Background Art
[0002] Faced with environmental problems such as global warming caused by excessive emissions of greenhouse gases such as carbon dioxide, humans urgently need to develop and utilize renewable clean energy. In order to achieve sustainable utilization and output of clean energy, energy storage technology has emerged. Among all energy storage technologies, lithium-ion batteries are widely used in energy storage, new energy vehicles, consumer electronics and other fields due to their high energy density, long cycle life, high voltage, small size and high safety.
[0003] During the first charge of a lithium-ion battery, the electrolyte will be reduced and decomposed on the surface of the negative electrode to form a solid electrolyte interface film (SEI film), which permanently consumes a large amount of lithium from the positive electrode, resulting in a low coulombic efficiency in the first cycle, reducing the capacity and energy density of the lithium-ion battery. Usually, lithium replenishment additives are added to the positive electrode material to replenish the electrode material with lithium to offset the irreversible lithium loss caused by the formation of the SEI film, which can effectively compensate for the first irreversible capacity loss of the battery. Organic lithium salts have high theoretical capacity and good air stability and are considered to be an attractive positive electrode pre-lithiation additive. However, due to their poor conductivity, their delithiation potential is high (>4.7V), which cannot match most commercial positive electrode materials, which greatly hinders their commercial application. Summary of the invention
[0004] The purpose of the present application is to provide a composite lithium supplement material and a preparation method and application thereof, aiming to solve the problem that the lithium supplement material has poor conductivity, high decomposition voltage, and is not conducive to being used as a lithium supplement additive.
[0005] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:
[0006] In a first aspect, the present application provides a composite lithium supplement material, comprising: a carbon core, a catalyst and a lithium-rich material, wherein the catalyst is distributed around the carbon core, and the lithium-rich material is distributed around the catalyst.
[0007] In a second aspect, the present application provides a method for preparing a composite lithium supplement material, comprising the following steps:
[0008] Providing a carbon core precursor;
[0009] The carbon core precursor is mixed with a lithium-rich material and a catalyst precursor, and subjected to a hydrothermal reaction, so that a catalyst intermediate formed by the catalyst precursor is distributed around the carbon core precursor, and the lithium-rich material is distributed around the catalyst intermediate, to obtain a composite lithium-supplementing material precursor;
[0010] The composite lithium-supplementing material precursor is calcined to obtain the composite lithium-supplementing material.
[0011] In a third aspect, the present application provides a positive electrode material, including the composite lithium-replenishing material of the present application and / or the composite lithium-replenishing material prepared by the preparation method of the composite lithium-replenishing material of the present application.
[0012] In a fourth aspect, the present application provides a secondary battery, comprising a positive electrode plate, a negative electrode plate and an electrolyte, wherein the positive electrode plate comprises the positive electrode material of the present application.
[0013] The composite lithium supplement material provided in the first aspect of the present application includes a carbon core, a catalyst and a lithium-rich material. Specifically, the catalyst is distributed around the carbon core, and the lithium-rich material is distributed around the catalyst. On the one hand, the carbon core can effectively improve the conductivity of the lithium-rich material, making it easier for the lithium-rich material to transfer electrons during the electrochemical reaction, thereby effectively enhancing the ability of the composite lithium supplement material to transmit lithium ions outward. On the other hand, the catalyst is distributed around the carbon core, which can reduce the risk of catalyst agglomeration, which is conducive to the catalyst to give full play to its catalytic performance, thereby effectively reducing the decomposition voltage of the lithium-rich material, improving the lithium-removal ability of the lithium-rich material, and enabling the composite lithium supplement material to give full play to its lithium supplement performance; on the other hand, the lithium-rich material is distributed around the catalyst, which is more conducive to the catalyst to exert its catalytic performance to reduce the decomposition voltage of the lithium-rich material and achieve efficient lithium supplementation. Therefore, the composite lithium supplement material provided by the present application has a lower decomposition voltage and excellent conductivity, and can release abundant lithium ions during the charge and discharge process, thereby achieving efficient lithium supplementation.
[0014] The preparation method of the composite lithium-supplementing material provided in the second aspect of the present application, through a hydrothermal reaction, the catalyst precursor forms a catalyst intermediate and is distributed around the carbon core precursor, while the lithium-rich material is distributed around the catalyst intermediate, and then calcined, thereby effectively preparing a composite lithium-supplementing material having the properties of the composite lithium-supplementing material of the present application as described above. In addition, the preparation method of the composite lithium-supplementing material of the present application can ensure that the structure and electrochemical properties of the prepared composite lithium-supplementing material are stable, so that the lithium-supplementing performance can be fully exerted, and the composite lithium-supplementing material is endowed with excellent lithium-removal ability, so as to achieve efficient lithium-supplementing of the battery, which is conducive to wide application.
[0015] The positive electrode material provided in the third aspect of the present application contains the composite lithium replenishing material of the present application, and the composite lithium replenishing material can delithium at a low delithiation voltage, has good stability, and has a high lithium replenishing capacity. It can replenish the lithium ions consumed by the SEI film during the first charge and discharge, thereby achieving efficient lithium replenishment, which is beneficial to improving the first cycle efficiency and reversible capacity of the manufactured lithium-ion battery.
[0016] The secondary battery provided in the fourth aspect of the present application contains the positive electrode material of the present application. Therefore, the secondary battery of the present application has high energy density and cycle performance, and stable electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0018] Figure 1 It is a schematic diagram of the structure of the composite lithium supplement material provided in the embodiment of the present application.
[0019] Among them, the reference numerals in the figure are:
[0020] 100, core, 200, shell;
[0021] 10. Carbon core, 20. Catalyst, 30. Lithium-rich material. DETAILED DESCRIPTION
[0022] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0023] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0024] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0025] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0026] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0027] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0028] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0029] In the description of the embodiments of the present application, SEI (solid electrolyte interface) membrane refers to a solid electrolyte phase interface membrane having the characteristics of a solid electrolyte, that is, a membrane formed by a passivation layer covering the surface of the electrode material when the electrode material and the electrolyte react at the solid-liquid interface during the first charge and discharge process of a liquid lithium-ion battery.
[0030] A first aspect of an embodiment of the present application provides a composite lithium supplement material, including a carbon core, a catalyst and a lithium-rich material, wherein the catalyst is distributed around the carbon core, and the lithium-rich material is distributed around the catalyst.
[0031] It is understandable that the composite lithium supplement material is added to the electrode and acts as a "sacrificial agent" during the first cycle of charging, releasing all the lithium ions it contains at one time as much as possible to replenish the irreversible lithium ions consumed by the formation of the SEI film at the negative electrode, thereby maintaining sufficient lithium ions in the battery system and improving the battery's initial efficiency and overall electrochemical performance.
[0032] The composite lithium supplement material provided in the first aspect of the embodiment of the present application includes a carbon core, a catalyst and a lithium-rich material, specifically: the catalyst is distributed around the carbon core, and the lithium-rich material is distributed around the catalyst. On the one hand, the carbon core has good electrical conductivity, which can effectively improve the electrical conductivity of the lithium-rich material, thereby effectively improving the migration rate of lithium ions contained in the lithium-rich material, thereby effectively enhancing the ability of the composite lithium supplement material to transmit lithium ions outward; on the other hand, the carbon core can be used as a carrier, that is, the catalyst is distributed around the carbon core, so that the risk of catalyst agglomeration can be reduced, which is conducive to the catalyst to give full play to its catalytic performance, thereby effectively reducing the decomposition voltage of the lithium-rich material, improving the lithium-removal ability of the lithium-rich material, and enabling the composite lithium supplement material to give full play to its lithium supplement performance; on the other hand, the lithium-rich material is distributed around the catalyst, which is more conducive to the catalyst to exert its catalytic performance to reduce the decomposition voltage of the lithium-rich material and achieve efficient lithium supplementation. Therefore, the composite lithium supplement material provided by the present application has a low decomposition voltage, excellent electrical conductivity and high structural stability, and can release abundant lithium ions during the charging and discharging process, thereby achieving efficient lithium supplementation.
[0033] The catalyst is distributed around the carbon core. In one embodiment, there may be a binding force between the catalyst and the carbon core. For example, the catalyst is bound to the outer layer of the carbon core. The catalyst may be directly bound to the outer surface of the carbon core or indirectly bound to the outer surface of the carbon core. In another embodiment, there is no binding force between the catalyst and the carbon core. For example, the catalyst contacts the carbon core.
[0034] The lithium-rich material is distributed around the catalyst. In one embodiment, there may be a binding force between the lithium-rich material and the catalyst. For example, the lithium-rich material is bound to the outer surface of the catalyst. The lithium-rich material may be directly bound to the outer surface of the catalyst or indirectly bound to the outer surface of the catalyst. In another embodiment, there is no binding force between the lithium-rich material and the catalyst. For example, the lithium-rich material is in contact with the catalyst.
[0035] Therefore, the composite lithium-replenishing material of the embodiment of the present application, through the ingredients contained and the interaction between the components, coupled with the specific structure, enables the components to play a synergistic role, allowing the composite lithium-replenishing material of the embodiment of the present application to provide more irreversible lithium ions during the first cycle, thereby improving its lithium-replenishing effect, and after completing the lithium-replenishing effect, it can also play the role of a conductive agent.
[0036] See also Figure 1 The composite lithium supplement material includes a carbon core 10 , a catalyst 20 and a lithium-rich material 30 . The catalyst 20 is distributed around the carbon core 10 , and the lithium-rich material 30 is distributed around the catalyst 20 .
[0037] In some embodiments, the catalyst includes catalyst nanoclusters that are grown in situ on the outer surface of the carbon core.
[0038] Catalyst nanoclusters have a high specific surface area, which is conducive to the full contact between lithium-rich materials and catalysts. This means that the catalyst and lithium-rich materials have a large contact area, which can effectively reduce the activation energy of the lithium-rich material delithiation reaction, improve its reaction activity, and effectively improve the capacity utilization of lithium-supplementing materials. In addition, catalyst nanoclusters can also accelerate the transmission rate of lithium ions, further effectively regulate the electronic structure and stability of active sites, enhance the charge transfer of the interface, and thus accelerate the delithiation reaction kinetics of lithium-rich materials.
[0039] Catalyst nanoclusters grow in situ on the outer surface of the carbon core. In this way, the carbon core, as a carrier of the catalyst nanoclusters, can greatly reduce the risk of catalyst agglomeration, which is beneficial for the catalyst to exert its catalytic effect, such as catalytic activity, catalytic selectivity and stability, thereby effectively reducing the decomposition voltage of lithium-rich materials.
[0040] In some embodiments, the catalyst nanoclusters have a petal-like morphology.
[0041] Catalyst nanoclusters with petal-shaped morphology have a larger specific surface area and a loose structure, which is more conducive to increasing the contact area between the catalyst nanoclusters and the lithium-rich material, thereby exerting the catalytic effect of the catalyst.
[0042] In some embodiments, the catalyst nanoclusters have a plurality of pores therein, and there are gaps between adjacent catalyst nanoclusters.
[0043] The catalyst nanocluster is formed by stacking and aggregating multiple catalyst nanosheets, so that not only does the catalyst nanocluster have several pores inside, but there are also certain gaps between adjacent catalyst nanoclusters. The gaps can provide sufficient space to effectively buffer the volume expansion of the composite lithium supplement material during the charge and discharge process, thereby improving the structural stability of the composite lithium supplement material.
[0044] There are gaps inside the catalyst nanoclusters and between adjacent nanoclusters. These gap structures can serve as overflow channels for gases generated by lithium-rich materials during the delithiation process, effectively inhibiting the volume expansion of the composite lithium-supplementing material caused by gas production, thereby protecting the stability of the composite lithium-supplementing material structure and greatly improving the safety performance of the battery.
[0045] In some embodiments, at least a portion of the lithium-rich material is attached to the outer surface of the catalyst nanoclusters.
[0046] Catalyst nanoclusters have a large specific surface area, which can provide a larger area for direct contact with lithium-rich materials. At this time, the lithium-rich materials are attached to the surface of the catalyst nanoclusters, which means that there is a large contact area between the catalyst and the lithium-rich material. Therefore, the decomposition voltage of the lithium-rich material can be effectively reduced, which is beneficial to the deintercalation of lithium ions and effectively improves the capacity utilization of the composite lithium-supplementing material.
[0047] In some embodiments, at least a portion of the lithium-rich material fills the pores of the catalyst nanoclusters.
[0048] Since the structure of the catalyst nanoclusters is loose, the lithium-rich material can be filled inside the structure of the catalyst nanoclusters, which means that the lithium-rich material and the catalyst have multi-directional direct contact, which is more conducive to the catalyst to play a catalytic role to reduce the decomposition voltage of the lithium-rich material, allowing the lithium-rich material to release sufficient active ions.
[0049] In some embodiments, at least a portion of the lithium-rich material fills the gaps between the catalyst nanoclusters.
[0050] The structure of the catalyst nanoclusters is loose, and there are certain gaps between adjacent catalyst nanoclusters, which are also filled with lithium-rich materials, so that the catalyst is in full contact with the lithium-rich material, which can effectively reduce the decomposition potential of the lithium-rich material, so as to better promote the delithiation of the lithium-supplementing material and reduce the delithiation potential of the lithium-supplementing material.
[0051] In some embodiments, the composite lithium-supplementing material further includes a shell layer, which is coated on the outer surface of the carbon core, the catalyst and the lithium-rich material.
[0052] The shell layer can effectively encapsulate the lithium-rich material and the catalyst, thereby isolating the lithium-rich material from external harmful substances, reducing the risk of side reactions between the catalyst and the electrolyte, and effectively stabilizing the interface between the lithium-supplementing material and the electrolyte, thereby improving the stability of the composite lithium-supplementing material. In addition, the lithium-rich material is confined between the carbon core and the shell layer, which can effectively alleviate the volume expansion of the lithium-rich material during the charging and discharging process, and has an additive improvement effect on improving the structural stability of the lithium-supplementing material.
[0053] In some embodiments, the shell layer includes a carbon material and nitrogen elements doped in the carbon material.
[0054] The carbon material has good electrical conductivity, and the shell layer formed thereby provides an excellent conductive environment for the lithium-rich material, thereby significantly improving the migration of lithium contained in the composite lithium-supplementing material, improving the capacity utilization rate of the lithium-rich material, and improving the lithium-supplementing effect of the composite lithium-supplementing material of the embodiment of the present application. In addition, the lithium-rich material is confined between the double carbon layers, that is, between the carbon core and the shell layer. Since the carbon core has excellent electrical conductivity and the shell layer also has excellent electrical conductivity, it can effectively shorten the transmission path of lithium ions and increase the rate of lithium ion deintercalation, which is beneficial for the lithium-rich material to give full play to its lithium-supplementing performance. After the composite lithium-supplementing material of the embodiment of the present application completes lithium replenishment, it can also play the role of a conductive agent.
[0055] The nitrogen element doped in the carbon material can provide abundant active sites, through which lithium ions can jump, thereby accelerating the transfer dynamics of lithium ions during the charging process and further improving the lithium removal ability of lithium-rich materials.
[0056] The coating material containing the doping element is coated on the outer layer of the carbon core, the catalyst and the lithium-rich material to form a shell layer, and the nitrogen element is located on the outer layer of the shell layer.
[0057] In some embodiments, the composite lithium supplement material includes a plurality of carbon cores, and the shell layer is coated on the periphery of the plurality of carbon cores.
[0058] See also Figure 1 The carbon core 10 , the catalyst 20 and the lithium-rich material 30 form a composite, the inner core 100 is composed of a plurality of carbon cores, and the shell layer 200 is coated on the outer surface of the inner core 100 .
[0059] The surface of the carbon core is combined with a catalyst, and the surface of the catalyst is combined with a lithium-rich material. The shell is coated on the periphery of the multiple carbon cores, which means that the multiple carbon cores form an inner core, and the shell is coated on the outer surface of the inner core. The surface of the carbon core is combined with a catalyst nanocluster, so that the carbon core has multiple pores inside, and there are also gaps between adjacent carbon cores, that is, the inner core formed by multiple carbon cores has a multi-void structure, which is conducive to the overflow of the gas generated by the lithium-rich material during the lithium stripping process, thereby protecting the integrity of the structure of the composite lithium supplement material.
[0060] The carbon core is used as a carrier, and the catalyst is combined on the outer surface of the carbon core, thereby improving the dispersion of the catalyst, reducing the risk of catalyst agglomeration, and being conducive to the catalytic effect of the catalyst; the combination of lithium-rich material and catalyst is conducive to the full contact between the catalyst and the lithium-rich material, which can effectively reduce the decomposition potential of the lithium-rich material, so as to better promote the delithiation of the lithium-supplementing material and reduce the decomposition potential of the lithium-supplementing material; at the same time, the carbon core can also provide a good conductive environment, which is more conducive to improving the conductivity of the lithium-rich material and is conducive to the delithiation of the lithium-rich material. In addition, the carbon core can also play a good protective and supporting role for the inner core, thereby improving the structural stability of the composite lithium-supplementing material.
[0061] In some embodiments, the carbon core comprises a carbon sphere.
[0062] The carbon core has a spherical or quasi-spherical structure, which is more conducive to the combination of catalysts on the surface of the carbon core.
[0063] In some embodiments, the particle size of the carbon core is 200 nm-600 nm. For example, the particle size of the carbon core can be 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 550 nm, 600 nm, etc., which are typical but non-limiting values.
[0064] The carbon core has a spherical or quasi-spherical structure. In this case, the particle size of the carbon core can be understood as the diameter of the carbon core.
[0065] Controlling the particle size of the carbon core within the above range is conducive to the attachment and / or growth of catalyst nanoclusters on its outer surface.
[0066] The carbon core has a non-smooth surface, that is, the surface of the carbon core is rough, which is more conducive to the growth of catalyst on the outer surface of the carbon core, thereby facilitating the attachment and / or growth of catalyst nanoclusters on its outer surface.
[0067] In some embodiments, the catalyst includes a transition metal oxide, such as an oxide corresponding to at least one of cobalt, nickel, and manganese.
[0068] The oxides corresponding to these metal elements can reduce the decomposition voltage of the lithium-rich material, thereby enabling the composite lithium-supplementing material to provide sufficient lithium ions, so that the composite lithium-supplementing material has a high capacity utilization rate.
[0069] Exemplary transition metal oxides include, but are not limited to, cobalt oxide (Co 3 O 4 ), nickel oxide (NiO), and manganese oxide (MnO).
[0070] In some embodiments, the particle size of the catalyst is 50 nm-200 nm. Exemplarily, the particle size of the catalyst can be 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, etc., which are typical but non-limiting values.
[0071] The embodiment of the present application controls the particle size of the catalyst within the above-mentioned range, which not only makes the catalyst have a larger surface area, thereby providing sufficient sites for the attachment of lithium-rich materials, which is beneficial to increase the contact area between the catalyst and the lithium-rich material, but also can shorten the transmission path of lithium ions, which is more beneficial to improve the transmission rate of lithium ions.
[0072] In some embodiments, the lithium-rich material includes an organic lithium salt.
[0073] These organic lithium salts have a relatively high decomposition voltage, such as Li2C2O4 (delithiation potential 4.7V), Li2O (delithiation potential 4.5V), Li2O2 (delithiation potential 4.3V), LiOH (delithiation potential 4.8V), Li4SiO4 (delithiation potential 4.5V), Li3PO4 (delithiation potential exceeding 4V), Li2CO3 (delithiation potential 4.7V), and Li5FeO4 (delithiation potential 4V). Therefore, these lithium-rich materials with relatively high decomposition voltages are difficult to compound with conventional positive electrode materials (such as lithium iron phosphate, whose delithiation potential is about 3.5V), which limits the widespread application of lithium-supplementing materials. Therefore, the present application confines the lithium-rich material and the catalyst between the double carbon layers, which can effectively reduce the decomposition voltage of the lithium-rich material, and can also effectively alleviate the expansion problem of the lithium-rich material during the charge and discharge process, thereby improving the utilization rate of these lithium-rich materials with relatively high decomposition voltages.
[0074] It can be understood that the delithiation potential refers to the potential required for lithium ions to be deintercalated from the positive electrode material during the battery charging process. Specifically, when the battery is charged, the lithium ions in the lithium supplement material will gradually break away from its lattice structure and move to the negative electrode through the electrolyte. The delithiation potential describes the potential value that the lithium supplement material needs to reach during this process.
[0075] In some embodiments, the lithium-rich material includes lithium oxalate.
[0076] In some embodiments, the D50 particle size of the lithium-rich material is 5 nm-100 nm. Exemplarily, the D50 particle size of the lithium-rich material can be 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, etc., which are typical but non-limiting values.
[0077] The D50 particle size is the particle size corresponding to when the cumulative particle size distribution percentage of the particles reaches 50%, and can be measured using methods known in the art.
[0078] The embodiment of the present application controls the D50 particle size of the lithium-rich material within the above range, which is conducive to the lithium-rich material adhering to the surface of the catalyst nanoclusters and / or filling in the internal gaps of the catalyst nanoclusters, thereby increasing the contact area between the lithium-rich material and the catalyst nanoclusters and effectively reducing the decomposition voltage of the lithium-rich material.
[0079] In some embodiments, the thickness of the shell layer is 5 nm to 50 nm. Exemplarily, the thickness of the shell layer can be 5 nm, 10 nm, 15 nm, 20 nm, 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, 50 nm, etc., which are typical but non-limiting values.
[0080] The embodiment of the present application optimizes and controls the thickness of the shell layer, so that the lithium-rich material in the composite lithium-supplementing material has a higher mass proportion and gives a higher lithium ion transmission rate, thereby promoting the lithium-supplementing performance of the lithium-rich material. In addition, within this thickness range, the shell layer can effectively encapsulate the lithium-rich material, catalyst, and carbon core, and on the basis of effectively improving the conductivity of the lithium-rich material, isolate the corrosion of the lithium-rich material by external harmful substances, thereby significantly improving the structural stability of the composite lithium-supplementing material.
[0081] In some embodiments, the specific surface area of the composite lithium supplement material is 400 to 800 m 2 / g. Exemplarily, the specific surface area of the composite lithium supplement material can be 400m 2 / g, 450m 2 / g、500m 2 / g, 550m 2 / g、600m 2 / g, 650m 2 / g、700m 2 / g, 750m 2 / g、800m 2 / g and other typical but non-limiting values.
[0082] Specific surface area refers to the total area per unit mass of a substance. In the embodiment of the present application, the specific surface area of the composite lithium supplement material is controlled within the above range, so that the surface of the composite lithium supplement material has sufficient active sites, thereby effectively improving the transmission rate of active ions. In addition, the lattice volume expansion of the composite lithium supplement material can be effectively reduced, further improving the structural stability of the composite lithium supplement material.
[0083] In some embodiments, the mass ratio of the lithium-rich material, the catalyst, and the carbon core is 100:1-10:5-25.
[0084] The role of the catalyst is to increase the reactivity of the lithium-rich material and reduce its reaction activation energy, so that the lithium-rich material has a lower decomposition voltage. Therefore, within the mass ratio of the catalyst provided in the embodiment of the present application, the catalytic effect of the catalyst is fully exerted, the decomposition voltage of the lithium-rich material is effectively reduced, and the capacity utilization rate of the lithium-rich material is improved. Exemplarily, the mass ratio of the catalyst can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, etc., which are typical but non-limiting values.
[0085] The role of the carbon core is not only to improve the conductivity of the lithium-rich material, but also to serve as a catalyst and a carrier of the lithium-rich material. In addition, the carbon element does not contribute lithium ions. Therefore, within the above-mentioned mass ratio of the carbon core, the composite lithium-supplementing material has excellent conductivity, high gram capacity and high structural stability. Exemplarily, the mass ratio of the carbon core can be 5, 8, 10, 12, 14, 16, 18, 20, 22, 25 and other typical but non-limiting values.
[0086] A second aspect of the present application provides a method for preparing a composite lithium supplement material, comprising the following steps:
[0087] Step S10, providing a carbon core precursor;
[0088] Step S20, mixing the carbon core precursor with the lithium-rich material and the catalyst precursor, and performing a hydrothermal reaction, so that the catalyst intermediate formed by the catalyst precursor is distributed around the carbon core precursor, and the lithium-rich material is distributed around the catalyst intermediate to obtain a composite lithium-supplementing material precursor;
[0089] Step S30: calcining the composite lithium-supplementing material precursor to obtain the composite lithium-supplementing material.
[0090] The preparation method of the composite lithium-supplementing material provided in the second aspect of the embodiment of the present application, through a hydrothermal reaction, the catalyst precursor forms a catalyst intermediate and is distributed around the carbon core precursor, while the lithium-rich material is distributed around the catalyst intermediate, and then calcined, thereby effectively preparing a composite lithium-supplementing material having the properties of the composite lithium-supplementing material of the present application as described above. In addition, the preparation method of the composite lithium-supplementing material of the present application can ensure that the structure and electrochemical properties of the prepared composite lithium-supplementing material are stable, so that the lithium-supplementing performance can be fully exerted, and the composite lithium-supplementing material is endowed with excellent lithium-removal ability, so as to achieve efficient lithium-supplementing of the battery, which is conducive to wide application.
[0091] In some embodiments, in step S10, the carbon core precursor includes a phenolic resin having a spherical or quasi-spherical structure.
[0092] Exemplarily, the carbon core precursor includes phenolic resin spheres.
[0093] In some embodiments, phenolic resin balls can be prepared by the following method:
[0094] Step S11, adding 3-aminophenol, formaldehyde solution and ammonia water to deionized water to form a mixed solution;
[0095] Step S12, adding acetone to the mixed solution obtained in step S11, stirring, and then performing solid-liquid separation, washing, and drying to obtain phenolic resin balls.
[0096] Specifically, in step S11, the mass concentration of ammonia water is 22% to 28 wt %. The function of ammonia water is to adjust the pH value in the mixed solution, which is conducive to the condensation reaction of 3-aminophenol and formaldehyde to form phenolic resin.
[0097] Specifically, in step S12, the stirring time is 6 hours to 18 hours. During the stirring process, 3-aminophenol and formaldehyde continue to undergo condensation reaction, and acetone helps to adjust the product to a spherical phenolic resin.
[0098] Specifically, in step S12, deionized water and ethanol are used for washing in sequence.
[0099] Specifically, in step S12, the drying temperature is 40°C-100°C.
[0100] In some embodiments, in step S20, the selection of lithium-rich material is as described above and will not be repeated here.
[0101] In some embodiments, in step S20, the catalyst precursor includes a soluble salt corresponding to a transition metal element, such as at least one of nitrates and acetates corresponding to the transition metal elements cobalt, nickel, and manganese.
[0102] In some embodiments, in step S20, the molar ratio of the lithium-rich material to the catalyst precursor is 100:2-20.
[0103] Within this ratio range, an appropriate amount of catalyst can be obtained to reduce the decomposition voltage of the lithium-rich material.
[0104] In some embodiments, in step S20, the raw material components for the hydrothermal reaction also include a carbon source. Exemplarily, the carbon source includes but is not limited to glucose.
[0105] In some embodiments, in step S20, the raw material components for the hydrothermal reaction further include a doping source. Exemplarily, the doping source includes but is not limited to urea.
[0106] In some embodiments, in step S20, the raw material components for the hydrothermal reaction further include a morphology control agent. Exemplarily, the morphology control agent includes but is not limited to ammonium fluoride (NH4F).
[0107] In some embodiments, in step S20, the molar ratio of the catalyst precursor, the carbon source, the doping source, and the morphology control agent is 1:1-5:3-10:1-5.
[0108] In some embodiments, in step S20, the steps of mixing the carbon core precursor with the lithium-rich material, the catalyst precursor and the carbon source to perform a hydrothermal reaction are specifically as follows:
[0109] Step S21, adding the carbon core precursor to a dispersant, and performing ultrasonic dispersion to obtain a dispersion;
[0110] Step S22, adding lithium-rich material, catalyst precursor, carbon source, doping source, and morphology control agent into the dispersion, stirring and transferring to a reactor for hydrothermal reaction, solid-liquid separation, washing, and drying to obtain a composite lithium-supplementing material precursor.
[0111] During the hydrothermal reaction, the catalyst precursor forms a transition metal hydroxide, i.e., a catalyst intermediate, and the lithium-rich material adheres to the surface of the catalyst intermediate. In this way, the lithium-rich material and the catalyst intermediate are tightly combined. The catalyst intermediate surrounds the carbon core precursor and grows in situ on the outer surface of the carbon core precursor to form an inner core composed of multiple primary particles, and the carbon source is coated on the outer surface of the inner core to form an initial shell.
[0112] Specifically, in step S21, the dispersant includes but is not limited to ethanol.
[0113] Specifically, in step S21, the ultrasonic dispersion time is 30 min-120 min.
[0114] Specifically, in step S22, the reaction kettle includes but is not limited to a tetrafluoroethylene hot press reaction kettle.
[0115] Specifically, in step S22, the conditions of the hydrothermal reaction are: temperature of 80°C-180°C, and time of 4h-12h.
[0116] Specifically, in step S22, deionized water and ethanol are used for washing in sequence.
[0117] Specifically, in step S22, the drying temperature is 40°C-100°C.
[0118] In some embodiments, in step S30, the calcination treatment conditions include calcination treatment at a temperature of 350° C.-550° C. for 2 h-5 h in an inert atmosphere.
[0119] After calcination, the carbon core precursor forms a carbon core, the initial shell forms a shell for covering the core, and the catalyst intermediate forms a catalyst that grows in situ on the outer surface of the carbon core, thus forming a composite lithium supplement material with a core-shell structure. Specifically: the catalyst in the core grows in situ on the outer surface of the carbon core, and the lithium-rich material adheres to the catalyst surface, that is, the lithium-rich material, the catalyst, and the carbon core are tightly combined to form a composite, which can give full play to the catalytic ability of the catalyst, reduce the catalyst content required in the composite material, and increase the content of the lithium-rich material in the composite lithium supplement material, thereby increasing the gram capacity of the composite lithium supplement material.
[0120] Exemplarily, the inert atmosphere includes at least one of nitrogen, argon, neon, and helium.
[0121] For example, the calcination temperature may be 350°C, 380°C, 400°C, 420°C, 450°C, 480°C, 500°C, 550°C, etc., which are typical but non-limiting values.
[0122] For example, the calcination time may be 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h, etc., which are typical but non-limiting values.
[0123] A third aspect of the embodiments of the present application provides a positive electrode material, including the composite lithium-replenishing material of the present application and / or a composite lithium-replenishing material prepared by the preparation method of the composite lithium-replenishing material of the present application.
[0124] The positive electrode material provided in the third aspect of the embodiment of the present application contains the composite lithium replenishing material of the present application, and the composite lithium replenishing material can delithium at a low delithiation voltage, has good stability, and has a high lithium replenishing capacity. It can replenish the lithium ions consumed by the SEI film during the first charge and discharge, thereby achieving efficient lithium replenishment, which is beneficial to improving the first cycle efficiency and reversible capacity of the manufactured lithium-ion battery.
[0125] A fourth aspect of an embodiment of the present application provides a secondary battery, which includes a positive electrode plate, a negative electrode plate and an electrolyte, wherein the positive electrode plate includes the positive electrode material of the present application; the electrolyte can be an electrolyte solution, in which case the secondary battery also includes a diaphragm arranged between the positive electrode plate and the negative electrode plate; or, the electrolyte can be a solid electrolyte solution, in which case the secondary battery does not have a diaphragm and is replaced by a solid electrolyte.
[0126] The secondary battery provided in the fourth aspect of the embodiment of the present application contains the positive electrode material of the present application. Therefore, the secondary battery of the present application has high energy density and cycle performance, and stable electrochemical performance.
[0127] In some embodiments, the positive electrode plate includes a positive current collector and a positive active layer bonded to at least one surface of the positive current collector, and the positive active layer includes the composite lithium replenishing material of the present application and / or the composite lithium replenishing material prepared by the preparation method of the composite lithium replenishing material of the present application.
[0128] The mass content of the above composite lithium supplementing material contained in the positive electrode active layer may be 0.01 wt % to 95 wt %.
[0129] The positive electrode active layer includes, in addition to the composite lithium supplement material, a binder and a conductive agent, wherein the binder can be a commonly used electrode binder, such as polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylonitrile copolymer, sodium alginate, chitosan and chitosan derivatives. In the embodiment of the present application, the conductive agent can be a commonly used conductive agent, such as one or more of graphite, carbon black, acetylene black, graphene, carbon fiber, C60 and carbon nanotubes.
[0130] In some embodiments, the positive electrode current collector includes but is not limited to at least one of aluminum foil, carbon-coated aluminum foil, iron foil, tin foil, zinc foil, nickel foil, titanium foil, and manganese foil.
[0131] In some embodiments, the positive electrode material includes a positive electrode active material, a conductive agent and a binder, that is, the composite lithium supplement material of the present application is directly used as a positive electrode active material, and is compounded with a conductive agent and a binder to prepare a positive electrode sheet.
[0132] The preparation process of the positive electrode plate can be: mixing the positive electrode active material, the conductive agent and the binder to obtain an electrode slurry, coating the electrode slurry on the positive electrode collector, and preparing the positive electrode plate through steps such as drying, rolling, and die cutting, wherein the positive electrode active material includes the composite lithium supplement material of the present application.
[0133] In some other embodiments, the positive electrode material includes a positive electrode active material, a lithium supplement, a conductive agent and a binder, that is, the composite lithium supplement material of the present application is used as a lithium supplement, and is compounded with the positive electrode active material, the conductive agent and the binder to prepare the positive electrode. The positive electrode active material includes but is not limited to lithium iron phosphate, lithium iron manganese phosphate, a ternary positive electrode material (such as NCM ternary or NCA ternary), a binary positive electrode material or a lithium-rich positive electrode material.
[0134] The preparation process of the positive electrode plate can be: mixing the positive electrode active material, the conductive agent, the binder and the lithium supplement agent to obtain an electrode slurry, coating the electrode slurry on the positive electrode collector, and preparing the positive electrode plate through steps such as drying, rolling, and die cutting, wherein the lithium supplement agent includes the composite lithium supplement material of the present application.
[0135] The following uses a number of specific embodiments to illustrate the composite lithium supplement material and its preparation method and application in the embodiments of the present application.
[0136] Composite lithium supplement material and preparation method thereof embodiment:
[0137] Example 1
[0138] A composite lithium supplement material, including a carbon core, a catalyst nanocluster (cobalt oxide nanocluster), a lithium-rich material (lithium oxalate) and a shell layer, wherein the catalyst nanocluster is in-situ grown on the outer surface of the carbon core, part of the lithium-rich material is attached to the outer surface of the catalyst nanocluster, part of the lithium-rich material is filled in the pores of the catalyst nanocluster, and part of the lithium-rich material is filled in the gaps between the catalyst nanocluster; the shell layer is coated on the periphery of multiple carbon cores, and the shell layer is also doped with nitrogen. The mass ratio of the lithium-rich material, the catalyst nanocluster and the carbon core is 100:5:10, the thickness of the shell layer is about 5nm, the particle size of the carbon core is about 500nm, and the particle size of the catalyst nanocluster is about 100nm.
[0139] A method for preparing a composite lithium supplement material comprises the following steps:
[0140] Step 1: Preparation of phenolic resin balls
[0141] 0.1 g of 3-aminophenol and 0.1 mL of HCHO solution were dissolved in 30 mL of deionized water, and ammonia water with a mass concentration of 28 wt % was added to obtain a mixed solution.
[0142] At 20°C, the mixed solution was stirred for 30 minutes, and then 10 mL of acetone was added and stirred for 12 hours. Then, solid-liquid separation was performed, and the product was washed with deionized water and ethanol respectively, and then the product was dried at 60°C to obtain phenolic resin balls.
[0143] Step 2: Preparation of composite lithium supplement material precursor
[0144] 0.5 g of phenolic resin balls were added into 60 mL of ethanol and ultrasonically dispersed for 2 h to obtain a dispersion.
[0145] 3 g of lithium oxalate, 2 mmol of cobalt nitrate hexahydrate (Co(NO3)2·6H2O), 10 mmol of urea, 6 mmol of ammonium fluoride (NH4F) and 5 mmol of glucose were added to the dispersion and stirred for 1 h, and then transferred to a polytetrafluoroethylene autoclave for hydrothermal reaction. The conditions of the hydrothermal reaction were 120°C / 8 h.
[0146] After the reaction was completed, the product was cooled to room temperature and then collected by centrifugation, rinsed with deionized water and ethanol three times, and dried at 60° C. for 12 h to obtain a composite lithium supplement material precursor.
[0147] Step 3: Preparation of composite lithium supplement materials
[0148] The composite lithium supplement material precursor was evenly ground and placed in an alumina crucible, and calcined at 400° C. for 3 h under a nitrogen atmosphere to obtain the composite lithium supplement material.
[0149] Example 2
[0150] A composite lithium supplement material, which differs from Example 1 in that: the combination mode of the lithium-rich material and the catalyst nanoclusters is different, and the lithium-rich material is attached to the outer surface of the catalyst nanoclusters. Specifically: the mass ratios of the lithium-rich material (lithium oxalate), the catalyst nanoclusters (cobalt tetroxide nanoclusters), and the carbon core are different. The mass ratio of the lithium-rich material (lithium oxalate), the catalyst nanoclusters (cobalt tetroxide nanoclusters), and the carbon core is 100:15:10, and the rest is the same as Example 1.
[0151] A method for preparing a composite lithium supplement material is different from that of Example 1 in that the amount of cobalt nitrate hexahydrate added in step 2 is 6 mmol, and the rest is the same as that of Example 1.
[0152] Example 3
[0153] A composite lithium supplement material, which differs from Example 1 in that: the combination mode of the lithium-rich material and the catalyst nanoclusters is different, the lithium-rich material is coated on the outer surface of the catalyst nanoclusters and filled in the gaps between the catalyst nanoclusters, specifically: the mass ratios of the lithium-rich material (lithium oxalate), the catalyst nanoclusters (cobalt tetroxide nanoclusters), and the carbon core are different, the mass ratio of the lithium-rich material (lithium oxalate), the catalyst nanoclusters (cobalt tetroxide nanoclusters), and the carbon core is 100:2:10, and the rest is the same as Example 1.
[0154] A method for preparing a composite lithium supplement material is different from that of Example 1 in that, in step 1, the amount of cobalt nitrate hexahydrate added in step 2 is 1 mmol, and the rest is the same as in Example 1.
[0155] Example 4
[0156] A composite lithium supplement material, which is different from Example 1 in that the morphology of the catalyst is different. Specifically, the morphology of the catalyst is granular, and the rest is the same as Example 1.
[0157] A method for preparing a composite lithium supplement material is different from that of Example 1 in that ammonium fluoride is not added in step 2, and the rest is the same as that of Example 1.
[0158] Example 5
[0159] A composite lithium supplement material is different from Example 1 in that the type of catalyst is different, specifically, the catalyst is nickel oxide nanoclusters, and the rest is the same as Example 1.
[0160] A method for preparing a composite lithium supplement material, which differs from Example 1 in that, in step 2, cobalt nitrate hexahydrate is replaced with nickel nitrate hexahydrate, and the rest is the same as Example 1.
[0161] Example 6
[0162] A composite lithium supplement material is different from Example 1 in that the particle size of the carbon core is different from that of the catalyst, specifically, the particle size of the carbon core is 2 μm, and the rest is the same as Example 1.
[0163] A method for preparing a composite lithium supplement material, which differs from Example 1 in that:
[0164] In step 1, the stirring time after adding acetone is 20 hours;
[0165] The rest is the same as in Example 1.
[0166] Example 7
[0167] A composite lithium supplement material is different from Example 1 in that the particle size of the carbon core is different from that of the catalyst. Specifically, the particle size of the carbon core is 200 nm. Others are the same as Example 1.
[0168] A method for preparing a composite lithium supplement material, which differs from Example 1 in that:
[0169] In step 1, the stirring time after adding acetone is 5 hours;
[0170] The rest is the same as in Example 1.
[0171] Example 8
[0172] A composite lithium supplement material, which differs from the embodiment 1 in that it does not include a shell layer. Specifically, the composite lithium supplement material includes a lithium-rich material (lithium oxalate), a catalyst nanocluster (cobalt oxide nanocluster) and a carbon core in a mass ratio of 100:5:10.
[0173] A method for preparing a composite lithium supplement material is different from that of Example 1 in that urea and glucose are not added in step 2, and the rest is the same as that of Example 1.
[0174] Step 2 is as follows:
[0175] 0.05 g of phenolic resin balls were added to 60 mL of ethanol and ultrasonically dispersed for 2 h to obtain a dispersion.
[0176] 6 g of lithium oxalate, 2 mmol of cobalt nitrate hexahydrate (Co(NO3)2·6H2O) and 6 mmol of ammonium fluoride (NH4F) were added to the dispersion and stirred for 1 h, and then transferred to a polytetrafluoroethylene autoclave for hydrothermal reaction at 120°C / 8 h.
[0177] After the reaction was completed, the product was cooled to room temperature and then collected by centrifugation, rinsed with deionized water and ethanol three times, and dried at 60° C. for 12 h to obtain a composite lithium supplement material precursor.
[0178] Comparative Example 1
[0179] This comparative example provides a composite lithium supplement material, which differs from Example 1 in that it does not include a carbon core. Specifically, the composite lithium supplement material includes a lithium-rich material (lithium oxalate) and a catalyst nanocluster (cobalt tetroxide nanocluster) in a mass ratio of 100:15, the catalyst nanocluster and the lithium-rich material are combined with each other, the shell layer is coated on the outer layer of the lithium-rich material and the catalyst nanocluster, the shell layer is also doped with nitrogen, the shell layer thickness is 5nm, and the rest is the same as Example 1.
[0180] A method for preparing a composite lithium supplement material is different from that of Example 1 in that no phenolic resin balls are added in step 2, and the rest is the same as that of Example 1.
[0181] Step 2 is as follows:
[0182] 6 g of lithium oxalate, 2 mmol of cobalt nitrate hexahydrate (Co(NO3)2·6H2O), 10 mmol of urea, 6 mmol of ammonium fluoride (NH4F) and 5 mmol of glucose were added to 60 mL of ethanol and stirred for 1 h, and then transferred to a polytetrafluoroethylene autoclave for hydrothermal reaction. The conditions of the hydrothermal reaction were 120°C / 8 h.
[0183] After the reaction was completed, the product was cooled to room temperature and then collected by centrifugation, rinsed with deionized water and ethanol three times, and dried at 60° C. for 12 h to obtain a composite lithium supplement material precursor.
[0184] Comparative Example 2
[0185] This comparative example provides a lithium supplement material, which only includes lithium oxalate.
[0186] Lithium-ion battery example:
[0187] The composite lithium supplement materials provided in Examples 1 to 8 and the lithium supplement materials provided in Comparative Examples 1 to 2 are respectively assembled into positive electrodes and lithium ion batteries according to the following methods:
[0188] Positive electrode: Under the same conditions, the composite lithium supplement material: SP (conductive carbon black): PVDF (polyvinylidene fluoride) are mixed in a mass ratio of 90:4:6, and N-methylpyrrolidone (NMP) is used as a solvent to mix the materials evenly to form a slurry, which is then evenly coated on the surface of the aluminum foil, rolled to a certain thickness, and vacuum dried at 110°C for 12 hours to form a positive electrode sheet; wherein the composite lithium supplement material is the composite lithium supplement material provided in the above-mentioned Examples 1 to 9 and the lithium supplement material provided in the comparative example.
[0189] Counter electrode: Lithium metal sheet.
[0190] Electrolyte: The electrolyte is a 1 mol / L LiPF6 / ethylene carbonate:ethyl methyl carbonate (volume ratio) = 1:1 solution.
[0191] Diaphragm: Polypropylene microporous membrane.
[0192] Lithium ion battery assembly: The lithium metal sheet-diaphragm-electrolyte-positive electrode sheet assembly sequence is assembled into a button-type lithium ion battery in an inert atmosphere glove box. The batteries containing the composite lithium supplement materials provided in Examples 1 to 8 are respectively recorded as Examples S1 to S8, and the batteries containing the lithium supplement materials provided in Comparative Examples 1 to 2 are recorded as Comparative Examples DS1 to DS2.
[0193] Performance Testing
[0194] (1) Powder resistivity
[0195] The resistivity of the positive electrode lithium supplement material in each embodiment and comparative example was calculated and tested by a four-probe method.
[0196] (2) Electrochemical performance test
[0197] The electrochemical properties of each lithium ion battery assembled in the above lithium ion battery embodiment were respectively tested as shown in Table 1, and the test conditions were as follows: charging at a rate of 0.1C, with a cut-off voltage of 4.7V; constant voltage charging at a cut-off of 4.7V; standing for 10 minutes after the charging process, discharging at a rate of 0.1C, with a cut-off voltage of 2.5V; observing the charging platform during the charging process to obtain the delithiation potential of the lithium supplement material.
[0198] The relevant performance test results of the composite lithium-rich material and lithium secondary battery are shown in Table 1 below.
[0199] Table 1 Related performance test results
[0200]
[0201]
[0202] From the results in Table 1, it can be seen that the powder resistivity of the composite lithium supplement materials prepared in Examples 1-8 is much lower than that in Comparative Examples 1-2, and the delithiation potential of the composite lithium supplement materials prepared in Examples 1-8 is lower than that in Comparative Examples 1-2. In the composite lithium supplement materials provided in the present application, the lithium-rich material obtains higher conductivity and ion transport properties by combining carbon cores and catalyst nanoclusters, thereby improving the conductivity of the lithium supplement material, solving the problem of high delithiation potential, and achieving the effect of catalytic delithiation.
[0203] It can be seen from Example 1 and Comparative Examples 1-2 in Table 1 that the addition of a conductive carbon core and the construction of an outer N-doped carbon shell layer can better catalyze the delithiation of lithium oxalate to achieve a better lithium replenishment effect. In Comparative Example 1, the composite material is composed only of a catalyst, lithium oxalate and a conductive carbon layer, and does not contain a conductive carbon core, resulting in poor conductivity, and the delithiation potential is still high, which is difficult to meet the actual application requirements. In Comparative Example 2, due to its large powder resistivity, the lithium oxalate has poor conductivity, which leads to the fact that it can only start to delithiate after reaching the 4.7V platform, and the delithiation is incomplete, resulting in a poor lithium replenishment effect.
[0204] From the comparison between Example 1 and Examples 2 and 4 in Table 1, it can be seen that the lithium supplement material in Example 1 has a better lithium supplement advantage. The reason is that the ratio of lithium oxalate to catalyst nanoclusters and carbon cores in Example 1 is relatively suitable, and lithium oxalate can be fully dispersed on the outer surface of the nanoclusters, in the pores of the nanoclusters, and in the gaps between the nanoclusters, ensuring that the catalyst and lithium oxalate are in full contact, thereby giving full play to the lithium supplement performance of the material. In Example 2, there are more nanoflower cluster catalysts grown in the composite lithium supplement material synthesized, and agglomeration and stacking will occur. The proportion of lithium oxalate is relatively small, and it can only adhere to the surface of the catalyst. The contact is not sufficient, thereby affecting the lithium de-lithiation effect of lithium oxalate. In Example 3, there are fewer nanoflower cluster catalysts synthesized, resulting in lithium oxalate being distributed in the gaps between the catalysts and also coated on the outer surface of the catalyst. In this case, a small amount of catalyst cannot catalyze the de-lithiation of a large amount of lithium oxalate.
[0205] From the comparison between Example 1 and Example 4 in Table 1, it can be seen that the catalyst in Example 1 has greater advantages in both lithium removal capacity and lithium removal potential. The reason is that the catalyst in Example 1 has a special morphology of nanoflower agglomeration, which can expose a larger surface area to fully contact with lithium oxalate to achieve the effect of amplifying the catalytic effect. The catalyst in Example 4 only presents the state of nanoparticles, with a small specific surface area. In addition, the granular catalyst is difficult to be evenly distributed on the carbon surface, prone to agglomeration and other phenomena, and is not sufficiently in contact with lithium oxalate, making it difficult to fully exert its catalytic ability.
[0206] From the comparison between Example 1 and Example 5 in Table 1, it can be seen that the catalyst in Example 1 has a greater catalytic advantage. Although the use of nickel oxide nanoclusters in Example 5 can reduce the lithium delithiation platform of lithium oxalate to a certain extent, compared with other examples, the platform is relatively high and the reduction in the lithium delithiation potential is not obvious. In this catalytic system, cobalt tetroxide has a better catalytic effect.
[0207] From the comparison of Example 1 and Examples 6-7 in Table 1, it can be seen that the suitable carbon core and catalyst size in Example 1 are more conducive to lithium delithiation of lithium oxalate and have more catalytic advantages. The reason is that the carbon core particle size in Example 6 is too large, which reduces the electrical conductivity of the system and makes lithium delithiation difficult. On the other hand, the excessively large particle size and poor dispersibility may cause the growth catalyst to grow discontinuously and unevenly on the surface of the carbon core, further affecting the contact effect between lithium oxalate and the catalyst. In Example 8, the carbon core diameter is too small, and it is easy to agglomerate during the hydrothermal reaction, which is not conducive to the subsequent growth process of the catalyst.
[0208] From the comparison between Example 1 and Example 8 in Table 1, it can be seen that the outer N-doped carbon shell in Example 1 can significantly improve the conductivity of the material and reduce the delithiation potential of the composite lithium supplement material from 4.3V to 4.10V, which plays a vital role. The reason is that N-doping can introduce more active sites, enhance the charge transfer at the interface, and accelerate the delithiation reaction kinetics of the material.
[0209] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A composite lithium supplement material, characterized in that: include: A carbon core, a catalyst and a lithium-rich material, wherein the catalyst is distributed around the carbon core, and the lithium-rich material is distributed around the catalyst.
2. The composite lithium supplement material according to claim 1, characterized in that: The catalyst includes catalyst nanoclusters, which are in-situ grown on the outer surface of the carbon core.
3. The composite lithium supplement material according to claim 2, characterized in that: The catalyst nano clusters have a plurality of pores therein, and there are gaps between adjacent catalyst nano clusters.
4. The composite lithium supplement material according to claim 3, characterized in that: At least part of the lithium-rich material is attached to the outer surface of the catalyst nanocluster; and / or at least part of the lithium-rich material is filled in the pores of the catalyst nanocluster; And / or, at least part of the lithium-rich material fills the gaps between the catalyst nanoclusters.
5. The composite lithium supplement material according to any one of claims 1 to 4, characterized in that: The composite lithium-supplementing material further includes a shell layer, and the shell layer is coated on the outer surface of the carbon core, the catalyst and the lithium-rich material.
6. The composite lithium supplement material according to claim 5, characterized in that: The shell layer includes a carbon material and a nitrogen element doped in the carbon material; and / or, the composite lithium supplement material includes a plurality of the carbon cores, and the shell layer is coated on the periphery of the plurality of the carbon cores; and / or, the thickness of the shell layer is 5nm-50nm.
7. The composite lithium supplement material according to any one of claims 1 to 4, characterized in that: The carbon core comprises a carbon sphere; and / or The catalyst comprises a transition metal oxide; and / or The particle size of the catalyst is 50nm-200nm; and / or The lithium-rich material comprises an organic lithium salt; and / or The D50 particle size of the lithium-rich material is 5nm-100nm; and / or The particle size of the carbon core is 200nm-600nm; and / or The specific surface area of the composite lithium supplement material is 400 to 800 m 2 / g; and / or The mass ratio of the lithium-rich material, the catalyst and the carbon core is 100:1-10:5-25.
8. A method for preparing a composite lithium supplement material, characterized in that: The following steps are involved: Providing a carbon core precursor; The carbon core precursor is mixed with a lithium-rich material and a catalyst precursor, and subjected to a hydrothermal reaction, so that a catalyst intermediate formed by the catalyst precursor is distributed around the carbon core precursor, and the lithium-rich material is distributed around the catalyst intermediate, to obtain a composite lithium-supplementing material precursor; The composite lithium-supplementing material precursor is calcined to obtain the composite lithium-supplementing material.
9. A positive electrode material, characterized in that: The invention comprises the composite lithium-supplementing material according to any one of claims 1 to 7 and / or the composite lithium-supplementing material prepared by the preparation method of the composite lithium-supplementing material according to claim 8.
10. A secondary battery, comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, characterized in that: The positive electrode sheet comprises the positive electrode material as claimed in claim 9.
Citation Information
Cited By
Sodium supplementing material and preparation method therefor, positive electrode sheet, and sodium-ion battery