Flat-plate-shaped ZSM-5 supported metal palladium catalyst as well as preparation method and application thereof

By preparing a flat plate-shaped ZSM-5 supported metal palladium catalyst, the problems of poor selectivity and low activity of existing catalysts are solved, efficient hydrogenation conversion of polycyclic aromatic hydrocarbons is achieved, and the utilization value of coal tar is enhanced.

CN118976533AActive Publication Date: 2024-11-19CHINA UNIV OF MINING & TECH

Patent Information

Application Number
CN202411270133.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-19
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

The existing polycyclic aromatic hydrocarbon hydrogenation catalysts have problems such as poor selectivity and low catalytic activity, which limits the conversion efficiency of high value-added chemicals of coal tar.

Method used

Using a preparation method of a flat plate-shaped ZSM-5 supported metal palladium catalyst, by mixing silicon source, deionized water and template agent at room temperature, adding aluminum source and ammonium fluoride, hydrothermal crystallization and calcination, forming active metal Palladium is loaded on the surface of flat plate-shaped ZSM-5 molecular sieve, simplifying the process and reducing costs.

Benefits of technology

High selectivity and activity were achieved, the naphthalene conversion rate reached 51.33%, and the anaphthalene conversion rate was as high as 95.83%. The catalytic activity was significantly improved in the catalytic hydrogenation reaction of polycyclic aromatic hydrocarbons and had good application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976533A_ABST
    Figure CN118976533A_ABST
Patent Text Reader

Abstract

The invention discloses a tabulate ZSM-5 supported metal palladium catalyst as well as a preparation method and application thereof. The catalyst comprises a tabulate ZSM-5 molecular sieve carrier and active metal palladium, the b-axis length of the tabulate ZSM-5 molecular sieve carrier is 50-60 nm, the active metal palladium is loaded on the surface of the tabulate ZSM-5 molecular sieve carrier, and the metal loading capacity is 0.1-2.0 wt%. The tabulate molecular sieve supported metal catalyst is synthesized by using an in-situ synthesis method, and the diffusion path is shortened by reducing the b-axis thickness of the ZSM-5 molecular sieve, so that the diffusion rate and the catalytic reaction effect are improved. The tabulate ZSM-5 supported metal palladium catalyst is used for a polycyclic aromatic hydrocarbon hydrogenation reaction, and under the conditions that the temperature is 200 DEG C, the pressure is 2 MPa, the H2 is adopted and the reaction is performed for 1 hour, the highest naphthalene conversion rate can reach 51.33%, and the acenaphthene conversion rate is as high as 95.83% through the tabulate ZSM-5 supported metal palladium catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal palladium catalysts and catalytic hydrogenation of polycyclic aromatic hydrocarbons, and in particular to a flat ZSM-5 supported metal palladium catalyst and a preparation method and application thereof. Background Art

[0002] Polycyclic aromatic hydrocarbons refer to a class of hydrocarbons including naphthalene-based bicyclic aromatic hydrocarbons and anthracene- and phenanthrene-based tricyclic aromatic hydrocarbons. Naphthalene oil is a separated product of the 200-230°C fraction of coal tar. 80-85% of naphthalene in coal tar exists in the naphthalene oil fraction. Naphthalene and acenaphthene are the main compounds in naphthalene oil. Selective hydrogenation of naphthalene into high value-added chemicals such as tetralin, decalin, tetralin, and decalin can greatly increase the utilization value of coal tar. At present, the catalysts used for the hydrogenation of polycyclic aromatic hydrocarbons have the disadvantages of poor selectivity and low catalytic activity. Therefore, the development of highly active and highly selective hydrogenation catalysts has become a key step in the hydrogenation conversion of polycyclic aromatic hydrocarbons.

[0003] In recent years, different approaches have been adopted to improve the accessibility and diffusion efficiency of ZSM-5 molecular sieves, generally by modifying the morphology and structure of molecular sieve crystals, such as reducing the crystals to nanometer size, introducing mesopores into the zeolite structure, and reducing the crystal thickness along special diffusion paths. Among them, shortening the b-axis thickness of ZSM-5 crystals, that is, reducing the diffusion path of reactants, has attracted much attention. The key milestone is the preparation of thin plate-type ZSM-5 nanosheets developed by Ryoo et al. However, the current synthesis of ZSM-5 molecular sieve nanosheets is hindered by its high cost, environmental unfriendliness, and complex organic structure directing agents (SDAs), which hinders its widespread application, especially limiting large-scale application in actual industry. Therefore, it is a very promising research to obtain such thin plate-type ZSM-5 zeolite using a synthetic system with readily available raw materials and easy operation. Summary of the invention

[0004] The first object of the present invention is to provide a method for preparing a flat ZSM-5 supported metal palladium catalyst, which has simple steps and can greatly reduce the amount of Pd used and the catalyst cost.

[0005] The second object of the present invention is to provide a flat ZSM-5 supported metal palladium catalyst prepared by the above preparation method.

[0006] The third object of the present invention is to provide the application of the above-mentioned flat ZSM-5 supported metal palladium catalyst.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] In a first aspect, the present invention provides a method for preparing a flat ZSM-5 supported metal palladium catalyst, comprising the following steps:

[0009] (1) mixing a silicon source, deionized water and a template at room temperature and stirring until a transparent synthetic gel is obtained, wherein the molar composition of the gel is SiO2 / template=1:0.35;

[0010] (2) adding an aluminum source to the gel obtained in step (1) and stirring at 90° C. for 12 h; the amount of the aluminum source added is maintained at nSiO2 / nAl2O3=1:(0.01-0.04);

[0011] (3) dissolving ammonium fluoride (NH4F) in deionized water, slowly adding it to the gel obtained in step (2) after ultrasonic treatment, and stirring vigorously for 12 h; the amount of ammonium fluoride added is maintained at nSiO2 / nNH4F=1:(0.1-1.0);

[0012] (4) hydrothermally crystallizing the gel obtained in step (3); after the crystallization reaction is completed, washing the obtained product with deionized water until it is neutral and then drying to obtain a molecular sieve solid powder;

[0013] (5) fully grinding the obtained molecular sieve solid powder and calcining to remove the template, thereby obtaining a flat ZSM-5 molecular sieve carrier;

[0014] (6) dissolving palladium acetate in dichloromethane, adding the flat ZSM-5 molecular sieve support thereto after ultrasonic treatment, stirring vigorously for 3 hours, and standing at room temperature for 24 hours; then, drying, calcining and reducing to obtain a flat ZSM-5 supported metal palladium (Pd) catalyst.

[0015] Preferably, the silicon source is selected from at least one of tetraethyl silicate (TEOS), silica sol, water glass, white carbon black and solid silica gel.

[0016] Preferably, the template agent is at least one selected from tetrapropylammonium hydroxide (TPAOH), tetramethylammonium hydroxide, tetraethylammonium hydroxide and tetrapropylammonium hydroxide.

[0017] Preferably, the aluminum source is selected from at least one of pseudo-boehmite (PB), sodium aluminate (NaAlO2), aluminum sulfate, aluminum chloride, aluminum nitrate, and aluminum isopropoxide.

[0018] Preferably, the crystallization temperature in step (4) is 160° C. and the crystallization time is 72 h.

[0019] Preferably, the calcination temperature in step (5) is 550° C. and the calcination time is 6 hours.

[0020] Preferably, in step (6), the drying temperature is 80-120°C and the drying time is 8-12h; the calcination temperature is 550°C and the calcination time is 4h; and the reduction refers to reduction under hydrogen conditions at 400°C for 2h.

[0021] In a second aspect, the present invention provides a flat ZSM-5 supported metal palladium catalyst prepared by the above preparation method.

[0022] The catalyst comprises a flat ZSM-5 molecular sieve carrier and active metal palladium. The b axis length of the flat ZSM-5 molecular sieve carrier is 50-60nm. The active metal palladium is loaded on the surface of the flat ZSM-5 molecular sieve carrier, and the metal loading amount is 0.1-2.0wt%.

[0023] In a third aspect, the present invention provides the use of the above-mentioned flat ZSM-5 supported metal palladium catalyst in the hydrogenation of polycyclic aromatic hydrocarbons.

[0024] The specific application steps include: adding the hydrogenation substrate naphthalene (or acenaphthene), Pd / ZSM-5 catalyst and n-hexane solvent into a tank reactor, sealing and introducing hydrogen three times to remove the residual air; then, pressurizing the reactor to 0.1-2.0MPa with hydrogen at room temperature, then heating to 180-240°C and maintaining it at a stirring speed of 800rpm for 1-2h. After the experiment, the reaction system is naturally cooled to room temperature and the pressure is released; the reaction mixture is filtered to remove the catalyst, and the obtained organic phase is analyzed by gas chromatography-mass spectrometry and gas chromatography.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. The flat ZSM-5 supported metal palladium catalyst synthesized by the present invention comprises a flat ZSM-5 molecular sieve carrier and an active metal palladium. The active metal palladium is supported on the surface of the flat ZSM-5 molecular sieve carrier. The flat ZSM-5 molecular sieve obtained by controlling the b-axis growth process of the flat ZSM-5 molecular sieve carrier by the proportion of ammonium fluoride solution during the synthesis process has a b-axis length of 50-60 nm.

[0027] 2. The flat ZSM-5 supported metal palladium catalyst synthesized by the present invention is used for the hydrogenation reaction of polycyclic aromatic hydrocarbons. Under the conditions of 200°C, 2MPa H2, and 1h reaction, the flat ZSM-5 supported metal palladium catalyst can make the naphthalene conversion rate reach up to 51.33% and the acenaphthene conversion rate reach up to 95.83%;

[0028] 3. The preparation process of the present invention is simple and easy to operate, improves the activity of catalytic hydrogenation, and has good application prospects in the catalytic hydrogenation reaction of polycyclic aromatic hydrocarbons. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 1 is the XRD diagram of the catalysts with different silicon-aluminum ratios prepared in Examples 1-4 of the present invention;

[0030] Figure 2 This is a SEM image of the catalyst with SiO2 / Al2O3=25 prepared in Example 1 of the present invention;

[0031] Figure 3 This is a SEM image of the catalyst with SiO2 / Al2O3=50 prepared in Example 2 of the present invention;

[0032] Figure 4 This is a SEM image of the catalyst with SiO2 / Al2O3=80 prepared in Example 3 of the present invention;

[0033] Figure 5 is a SEM image of the catalyst with SiO2 / Al2O3=100 prepared in Example 4 of the present invention;

[0034] Figure 6 is the Py-IR graph of the catalysts with different silicon-aluminum ratios prepared in Examples 1-4 of the present invention at 473K;

[0035] Figure 7 is the Py-IR graph of the catalysts with different silicon-aluminum ratios prepared in Examples 1-4 of the present invention at 623K;

[0036] Figure 8 FT-IR images of catalysts with different silicon-aluminum ratios prepared in Examples 1-4 of the present invention;

[0037] Fig. 9 This is a diagram of the six isomers of perhydroacenaphthene. DETAILED DESCRIPTION

[0038] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0039] Example 1-4 The acidity of the planar ZSM-5 was adjusted to prepare plate-shaped catalysts loaded with metallic palladium and having different silicon-aluminum ratios.

[0040] Example 1

[0041] 14.608g TEOS, 10g deionized water and 19.965g TPAOH were mixed at room temperature and stirred for 1.5h to obtain a transparent synthetic gel, and then 0.372g PB was added to the obtained gel. Stirred for 12h at 90°C. After that, 2.164g NH4F was dissolved in 12.892g water, slowly added to the above gel after ultrasonication for 5min, and then the gel was vigorously stirred for 12h. The obtained gel was crystallized in an autoclave at 160°C for 3 days. After that, after the crystallization reaction was completed, the mixed solution was washed with deionized water until neutral and then dried to obtain a molecular sieve solid powder, which was then calcined at 550°C for 6h to finally obtain a flat ZSM-5 molecular sieve.

[0042] The flat ZSM-5 supported metal palladium catalyst was prepared by impregnation method. 0.0106g of palladium acetate was dissolved in 20mL of dichloromethane, and then 1g of flat ZSM-5 molecular sieve was added, stirred for 3h, and allowed to stand at room temperature for 24h. Then, it was dried at 80℃ for 12h, calcined at 550℃ for 4h, and finally reduced at 400℃ for 2h under hydrogen conditions to obtain a flat ZSM-5 supported metal palladium catalyst, named Pd / ZSM-5-25.

[0043] Example 2

[0044] 14.654g TEOS, 10g deionized water and 20.027g TPAOH were mixed at room temperature and stirred for 1.5h to obtain a transparent synthetic gel, and then 0.187g PB was added to the obtained gel. Stirred for 12h at 90°C. After that, 2.171g NH4F was dissolved in 12.963g water, slowly added to the above gel after ultrasonication for 5min, and then the gel was vigorously stirred for 12h. The obtained gel was crystallized in an autoclave at 160°C for 3 days. After that, after the crystallization reaction was completed, the mixed solution was washed with deionized water until neutral and then dried to obtain a molecular sieve solid powder, which was then calcined at 550°C for 6h to finally obtain a plate-like ZSM-5 molecular sieve.

[0045] The plate-shaped ZSM-5 supported metal palladium catalyst was prepared by impregnation method. 0.0106g of palladium acetate was dissolved in 20mL of dichloromethane, and then 1g of plate-shaped ZSM-5 molecular sieve was added, stirred for 3h, and allowed to stand at room temperature for 24h. Then, it was dried at 100℃ for 10h, calcined at 550℃ for 4h, and finally reduced at 400℃ for 2h under hydrogen conditions to obtain a plate-shaped ZSM-5 supported metal palladium catalyst, named Pd / ZSM-5-50.

[0046] Example 3

[0047] 14.670g TEOS, 10g deionized water and 20.049g TPAOH were mixed at room temperature and stirred for 1.5h to obtain a transparent synthetic gel, and then 0.117g PB was added to the obtained gel. Stirred for 12h at 90°C. After that, 2.174g NH4F was dissolved in 12.989g water, slowly added to the above gel after ultrasonication for 5min, and then the gel was vigorously stirred for 12h. The obtained gel was crystallized in an autoclave at 160°C for 3 days. After that, after the crystallization reaction was completed, the mixed solution was washed with deionized water until neutral and then dried to obtain a molecular sieve solid powder, which was then calcined at 550°C for 6h to finally obtain a plate-like ZSM-5 molecular sieve.

[0048] The plate-shaped ZSM-5 supported metal palladium catalyst was prepared by impregnation method. 0.0106g of palladium acetate was dissolved in 20mL of dichloromethane, and then 1g of plate-shaped ZSM-5 molecular sieve was added, stirred for 3h, and allowed to stand at room temperature for 24h. Then, it was dried at 120℃ for 10h, calcined at 550℃ for 4h, and finally reduced at 400℃ for 2h under hydrogen conditions to obtain a plate-shaped ZSM-5 supported metal palladium catalyst, named Pd / ZSM-5-80.

[0049] Example 4

[0050] 14.676g TEOS, 10g deionized water and 20.058g TPAOH were mixed at room temperature and stirred for 1.5h to obtain a transparent synthetic gel, and then 0.093g PB was added to the obtained gel. Stirred for 12h at 90°C. After that, 2.164g NH4F was dissolved in 12.998g water, slowly added to the above gel after ultrasonication for 5min, and then the gel was vigorously stirred for 12h. The obtained gel was crystallized in an autoclave at 160°C for 3 days. After that, after the crystallization reaction was completed, the mixed solution was washed with deionized water until neutral and then dried to obtain a molecular sieve solid powder, which was then calcined at 550°C for 6h to finally obtain a plate-like ZSM-5 molecular sieve.

[0051] The plate-shaped ZSM-5 supported metal palladium catalyst was prepared by impregnation method. 0.0106g of palladium acetate was dissolved in 20mL of dichloromethane, and then 1g of plate-shaped ZSM-5 molecular sieve was added, stirred for 3h, and allowed to stand at room temperature for 24h. Then, it was dried at 120℃ for 12h, calcined at 550℃ for 4h, and finally reduced at 400℃ for 2h under hydrogen conditions to obtain a plate-shaped ZSM-5 supported metal palladium catalyst, named Pd / ZSM-5-100.

[0052] The XRD patterns of the catalysts prepared in Examples 1-4 are as follows: Figure 1 As shown. By comparison, it was found that the characteristic diffraction peaks of ZSM-5 7.96o, 8.82o, 23.27o, 23.97o and 24.43o existed in the catalysts with different silicon-aluminum ratios, but the crystallinity of the four catalysts was quite different. Among them, the crystallinity of the plate-like ZSM-5 molecular sieve in the Pd / ZSM-5-25 catalyst was poor, and the crystallinity of the plate-like ZSM-5 molecular sieve in the Pd / ZSM-5-50 catalyst was the best.

[0053] The SEM images of the catalysts prepared in Examples 1-4 are as follows: Figure 2-Figure 5 As shown. Figure 2-Figure 5 It was found that the ZSM-5 molecular sieves in the Pd / ZSM-5-x catalysts all showed a thin plate structure. Figure 4 The b-axis length of the medium-plate ZSM-5 molecular sieve is about 50nm, but Figure 2 The morphology and structure are poor, which is consistent with the XRD results of Example 1.

[0054] The Py-IR patterns of the catalysts prepared in Examples 1-4 are as follows: Figure 6 , Figure 7 The Py-IR acidity results of catalysts with different Si / Al ratios are shown in Table 1. Comparing Examples 1-4, it is found that at 200°C and 350°C, Examples 1-4 have a low Py-IR acidity at 1450 cm -1 and 1540cm -1 The peak area at gradually decreases with the increase of silicon-aluminum ratio. At 200°C, the acid content of Pd / ZSM-5-25 (Example 1) is the highest, with B acid reaching 0.861 mmol / g and L acid being 0.173 mmol / g. The B acid in the series of catalysts prepared in Examples 1-4 is more than the L acid, proving that most of the aluminum is in the zeolite framework.

[0055] Table 1 Acidity evaluation results of catalysts with different Si-Al ratios

[0056]

[0057] The FT-IR images of the catalysts prepared in Examples 1-4 are as follows: Figure 8 As shown. The flat ZSM-5 molecular sieves are all at 800cm -1 、1099cm -1 and 1230cm -1 The asymmetric stretching vibration peak of SiO4 tetrahedral unit is shown. 1099cm -1 The peak at is attributed to the asymmetric stretching vibration of Si-OT (T represents Si or Al). However, with the increase of SiO2 / Al2O3 ratio, this peak gradually moves to higher wavenumbers.

[0058] Example 5-6: The catalyst prepared in the above examples 1-4 is applied to the catalytic hydrogenation reaction of condensed aromatic hydrocarbons naphthalene and acenaphthene.

[0059] Example 5

[0060] In a typical experiment, 100 mg of naphthalene, 50 mg of catalyst and 20 mL of n-hexane solvent were placed in a reactor. After sealing, H2 was introduced three times to remove residual air, and the reactor was checked for sealing. Subsequently, the reactor was pressurized to 0.1-2.0 MPa with hydrogen at room temperature, then heated to 180-240°C and maintained at a stirring speed of 800 rpm for 1-2 h. After the experiment, the reaction system was naturally cooled to room temperature and the pressure was released; the reaction mixture was filtered to remove the catalyst, and the obtained organic phase was analyzed by gas chromatography-mass spectrometry and gas chromatography.

[0061] Table 2 shows the data of the catalysts prepared in Examples 1-4 at an initial pressure of 2.0 MPa, a reaction temperature of 200° C., and a stirring speed of 800 rpm for 1 hour.

[0062] Table 2 Evaluation results of naphthalene hydrogenation catalyzed by catalysts with different acidity

[0063]

[0064] The evaluation results of naphthalene hydrogenation catalyzed by catalysts of different acidity are shown in Table 2. The catalytic activity of the catalyst shows a decreasing trend with the increase of the silicon-aluminum ratio. The Pd / ZSM-5-25 catalyst prepared in Example 1 makes the naphthalene conversion rate reach 51.33%, and the selectivity of decalin reaches 17.71%, and trans-decalin is generated with high selectivity, and the product contains only a very small amount of cis-decalin. The results show that the acidity of the carrier has a great influence on the catalyst performance. Appropriate acidity can effectively improve the hydrogenation activity of the catalyst, thereby improving the conversion rate of naphthalene and the selectivity of decalin.

[0065] Example 6

[0066] In a typical experiment, 100 mg of acenaphthene, 50 mg of catalyst, and 20 mL of n-hexane solvent were placed in a reactor. After sealing, H2 was introduced three times to remove residual air, and the sealing of the reactor was checked. Subsequently, the reactor was pressurized to 0.1-2.0 MPa with hydrogen at room temperature, and then heated to 180-240°C and maintained at a stirring speed of 800 rpm for 1-2 hours. After the experiment, the reaction system was naturally cooled to room temperature and the pressure was released; the reaction mixture was filtered to remove the catalyst, and the obtained organic phase was analyzed by gas chromatography-mass spectrometry and gas chromatography.

[0067] Table 3 shows the data of the catalysts prepared in Examples 1-4 at an initial pressure of 2.0 MPa, a reaction temperature of 200° C., and a stirring speed of 800 rpm for 1 hour.

[0068] Table 3 Evaluation results of acenaphthene hydrogenation catalyzed by catalysts with different acidity

[0069]

[0070] The evaluation results of acenaphthene hydrogenation catalyzed by catalysts of different acidity are shown in Table 3. The catalytic performance of the catalysts gradually decreases with the increase of the silicon-aluminum ratio, among which the Pd / ZSM-5-25 catalyst prepared in Example 1 has the strongest hydrogenation performance, making the conversion rate of acenaphthene reach 95.83%, and the selectivity of decahydroacenaphthene is as high as 36.99%.

[0071] The decahydroacenaphthene in Table 3 was analyzed and the six isomers of decahydroacenaphthene were as follows: Fig. 9 The proportions of the six substances in decahydroacenaphthene are analyzed, as shown in Table 4.

[0072] Table 4 Isomerization composition of perhydroacenaphthene

[0073]

[0074] Acenaphthene is deeply hydrogenated to form perhydroacenaphthene. There are six stereoisomers in perhydroacenaphthene. Since they appear in sequence according to the boiling point of the substance in the gas chromatograph, when the retention time is smaller, the boiling point is lower and the density is smaller, which belongs to the trans stereoisomer product. As the retention time is prolonged, the boiling point of the substance is higher, which belongs to the cis stereoisomer. Therefore, according to the peak order of the substance in the gas chromatograph, the six stereoisomers are represented by numbers 1-6. When acenaphthene is saturated and hydrogenated by different catalysts, the distribution of isomers of perhydroacenaphthene is shown in Table 4. It can be found from Table 4 that this series of catalysts selectively catalyzes the deep hydrogenation of acenaphthene to produce substance 3, and the highest percentage of substance 3 can reach 51.37%.

[0075] Example 7

[0076] The Pd / ZSM-5-25 prepared in Example 1 with the best hydrogenation performance was compared with a catalyst using commercial block ZSM-5-25 as a carrier, wherein the Pd metal loading method and loading amount were the same as those in Example 1.

[0077] The hydrogenation substrate naphthalene, catalyst and n-hexane solvent were added to a tank reactor, which was sealed and hydrogen was introduced three times to remove the residual air; then, the reactor was pressurized to 0.1-2.0 MPa with hydrogen at room temperature, and then the temperature was raised to 180-240°C and maintained at a stirring speed of 800 rpm for 1-2 hours. After the experiment, the reaction system was naturally cooled to room temperature and the pressure was released; the reaction mixture was filtered to remove the catalyst, and the obtained organic phase was analyzed by gas chromatography-mass spectrometry and gas chromatography.

[0078] Table 5 shows the data obtained when the two catalysts were kept at an initial pressure of 2.0 MPa, a reaction temperature of 200°C, and a stirring speed of 800 rpm for 1 hour.

[0079] Table 5 Evaluation results of naphthalene hydrogenation catalyzed by different catalysts

[0080]

[0081] The research results show that, comparing the reaction performance of Example 1 and commercial block ZSM-5-25, both of which have a silicon-aluminum ratio of 25, the conversion rate of Example 1 is 51.33%, which is much higher than 26.18% of commercial ZSM-5-25, proving that under the same acidic conditions, the diffusion effect of the flat molecular sieve is higher than that of the commercial block ZSM-5-25, which is beneficial to the diffusion of the macromolecular reactant naphthalene and the hydrogenation product, and improves the activity of catalytic hydrogenation.

[0082] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a flat ZSM-5 supported metal palladium catalyst, characterized in that: The following steps are involved: (1) mixing a silicon source, deionized water and a template at room temperature and stirring until a transparent synthetic gel is obtained, wherein the molar composition of the gel is SiO2 / template=1:0.35; (2) adding an aluminum source to the gel obtained in step (1) and stirring at 90° C. for 12 h; the amount of the aluminum source added is maintained at nSiO2 / nAl2O3=1:(0.01-0.04); (3) dissolving ammonium fluoride in deionized water, slowly adding it to the gel obtained in step (2) after ultrasonication, and stirring vigorously for 12 hours; the amount of ammonium fluoride added is maintained at nSiO2 / nNH4F=1:(0.1-1.0); (4) hydrothermally crystallizing the gel obtained in step (3); after the crystallization reaction is completed, washing the obtained product with deionized water until it is neutral and then drying to obtain a molecular sieve solid powder; (5) fully grinding the obtained molecular sieve solid powder and calcining to remove the template, thereby obtaining a flat ZSM-5 molecular sieve carrier; (6) dissolving palladium acetate in dichloromethane, adding the flat ZSM-5 molecular sieve support thereto after ultrasonication, stirring vigorously for 3 hours, and standing at room temperature for 24 hours; then, drying, calcining and reducing to obtain a flat ZSM-5 supported metal palladium catalyst.

2. The method for preparing a flat ZSM-5 supported metal palladium catalyst according to claim 1, wherein: The silicon source is selected from at least one of tetraethyl silicate, silica sol, water glass, white carbon black and solid silica gel; the template is selected from at least one of tetrapropylammonium hydroxide, tetramethylammonium hydroxide, tetraethylammonium hydroxide and tetrapropylammonium hydroxide; the aluminum source is selected from at least one of pseudo-boehmite, sodium aluminate, aluminum sulfate, aluminum chloride, aluminum nitrate and aluminum isopropoxide.

3. The method for preparing a flat ZSM-5 supported metal palladium catalyst according to claim 1, wherein The crystallization temperature in step (4) is 160° C. and the crystallization time is 72 h.

4. The method for preparing a flat ZSM-5 supported metal palladium catalyst according to claim 1, wherein The calcination temperature in step (5) is 550° C. and the calcination time is 6 hours.

5. The method for preparing a flat ZSM-5 supported metal palladium catalyst according to claim 1, wherein: In step (6), the drying temperature is 80-120° C. and the drying time is 8-12 hours; the calcination temperature is 550° C. and the calcination time is 4 hours; and the reduction refers to reduction under hydrogen conditions at 400° C. for 2 hours.

6. A flat ZSM-5 supported metal palladium catalyst prepared by the preparation method according to any one of claims 1 to 5.

7. The flat ZSM-5 supported metal palladium catalyst according to claim 6, characterized in that The catalyst comprises a flat ZSM-5 molecular sieve carrier and active metal palladium, wherein the active metal palladium is loaded on the surface of the flat ZSM-5 molecular sieve carrier, the b axis length of the flat ZSM-5 molecular sieve carrier is 50-60nm, and the metal loading amount is 0.1-2.0wt%.

8. Use of the flat ZSM-5 supported metal palladium catalyst according to claim 6 in the hydrogenation of polycyclic aromatic hydrocarbons.

9. The use according to claim 8, characterized in that The polycyclic aromatic hydrocarbon is naphthalene or acenaphthene.

10. The use according to claim 8, characterized in that The reaction temperature of the polycyclic aromatic hydrocarbon hydrogenation is 180-240° C.; the reaction pressure is 0.1-2 MPa; and the reaction time is 1-2 h.

Citation Information

Patent Citations

  • Synthesis method of hierarchical porous ZSM-5 molecular sieve anchored palladium nanoparticles

    CN110038627A

  • Preparation method of hollow molecular sieve catalyst and application of hollow molecular sieve catalyst in preparation of high-density aviation fuel by hydrogenation of polycyclic aromatic hydrocarbon

    CN113368891A

  • ZSM-5 molecular sieve as well as preparation method and application thereof

    CN119038575A

Cited By

  • HZSM-5 molecular sieve as well as preparation method and application thereof

    CN119702057A

  • Dry glue water heating method for synthesizing sheet type ZSM-5 zeolite

    CN120440910A