Honeycomb type Mn-Cu-M ternary composite metal oxide catalyst with high sulfur resistance as well as preparation method and application of honeycomb type Mn-Cu-M ternary composite metal oxide catalyst

By introducing interface regulators Cu and M into the catalyst, the interface structure of Mn-Cu-M ternary composite metal oxide is optimized, and the existing catalyst activity is insufficient and SO2 adsorption inhibition problems are solved, and efficient CO removal and low-temperature operation are achieved. Suitable for industrial flue gas purification, reducing energy consumption and pollution.

CN118976543APending Publication Date: 2024-11-19EAST CHINA UNIV OF SCI & TECH

Patent Information

Application Number
CN202410974488.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing catalysts are insufficient in the CO removal process and have poor adsorption inhibition effect on SO2, which limits the efficiency and cost-effectiveness of industrial flue gas purification.

Method used

Using honeycomb high sulfur-resistant Mn-Cu-M ternary metal oxide catalyst, nanorod-shaped Mn monomer metal oxide is synthesized by hydrothermal method, and interface regulators Cu and M are introduced to optimize their lattice distortion and interlayer Dislocation promotes the activation of CO and O2 and inhibits the adsorption of SO2.

Benefits of technology

It significantly improves the catalytic efficiency of CO oxidation, achieves a CO conversion rate of 90% at low temperatures, demonstrates excellent catalytic performance and anti-toxic properties, and is suitable for flue gas purification in industrial processes such as steel industry and waste incineration power generation boilers, reducing Energy consumption and pollutant emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976543A_ABST
    Figure CN118976543A_ABST
Patent Text Reader

Abstract

The invention discloses a honeycomb type high-sulfur-resistance Mn-Cu-M ternary composite metal oxide catalyst and a preparation method and application thereof.The catalyst is obtained in the mode that an active metal component A and an interface regulating agent B are introduced in sequence, the active metal component A is Mn, and the interface regulating agent B comprises Cu and M; the preparation method is different from a traditional one-step method, and synthesis of MnOx and introduction of interface regulators Cu and M are achieved through a two-step method. A catalyst grain boundary engineering strategy is adopted, an active metal component Mn and interface regulators Cu and M are introduced step by step, and the composite metal oxide catalyst with interface characteristics such as lattice distortion and interlayer dislocation is constructed. By accurately regulating and controlling the interface structure, activation of CO and O2 can be promoted to inhibit adsorption of SO2, so that the catalytic efficiency of CO oxidation is greatly improved, CO in byproduct flue gas in the industrial production process is efficiently removed at low temperature, and safety, environmental protection, energy conservation and emission reduction are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and in particular relates to a honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst and a preparation method and application thereof. Background Art

[0002] Carbon monoxide (CO), as a flammable and explosive gas, is an atmospheric pollutant that cannot be ignored and poses a serious threat to the environment and human health. CO mainly comes from the incomplete combustion of inferior fuels at low temperatures, and is commonly found in industrial flue gases produced by industrial processes such as steel sintering, biomass, lime kilns, and waste incineration power generation boilers. The concentration of CO in these industrial flue gases can reach 0.5% to 1%, which not only causes environmental pollution, but also is a waste of energy. It must be purified and removed to meet the standards before it can be discharged. In addition, CO removal technology plays a key role in many fields, such as hydrogen purification, catalyst detoxification process, and the development of CO gas detectors. Therefore, the removal of CO is not only crucial to improving air quality and protecting human health, but also a key link in promoting sustainable industrial development and promoting the advancement of environmental protection technologies.

[0003] Existing methods for removing CO mainly include physical adsorption, catalytic oxidation and plasma. Among them, although the physical adsorption method is easy to operate, its effect is often limited by the capacity and adsorption rate of the adsorption material; the plasma method is limited by its complex operation process and high equipment requirements. In contrast, the catalytic oxidation method has become the most direct and effective means of removing CO with its advantages of low energy consumption, no secondary pollution and easy operation. It is worth mentioning that the heat released during the catalytic oxidation process can effectively increase the flue gas temperature, which not only helps to remove CO, but also provides convenience for the subsequent treatment of industrial flue gas. In the catalytic oxidation method, the choice of catalyst is a key factor affecting the efficiency and cost of CO removal.

[0004] At present, precious metal catalysts, such as platinum (Pt), palladium (Pd), rhodium (Rh) and gold (Au), are known for their high catalytic efficiency, but their high cost and limited resource reserves restrict their popularity in large-scale applications. Non-precious metal catalysts, especially oxides and composite metal oxides composed of elements such as copper (Cu), manganese (Mn), cobalt (Co) and nickel (Ni), have attracted much attention due to their high cost-effectiveness and environmental friendliness, and are gradually becoming a hot spot in research and application. In the research field of non-precious metal catalysts, the manganese oxide series has attracted much attention due to its variable valence states and unique catalytic properties. Manganese oxide (MnO), manganese dioxide (MnO2), manganese trioxide (Mn2O3) and manganese tetraoxide (Mn3O4) constitute this family, among which manganese dioxide stands out for its excellent catalytic activity. Despite this, the activity of unmodified manganese oxide catalysts in catalytic reactions still has room for improvement. In order to overcome this limitation, researchers have explored a variety of modification methods and need to develop a new type of non-precious metal catalyst for the removal of CO from by-product flue gas in industrial production processes. Summary of the invention

[0005] In order to overcome the above-mentioned deficiencies in the prior art, the present invention provides a honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst and a preparation method thereof, which adopts a catalyst grain boundary engineering strategy, introduces active metal components Mn and interface regulators Cu and M in steps, and directionally optimizes interface properties such as lattice distortion and interlayer dislocation, promotes the activation of CO and O2 and inhibits the adsorption of SO2, thereby greatly improving the catalytic efficiency of CO oxidation, and efficiently removing CO from by-product flue gas in industrial production processes at low temperatures, thereby achieving safety, environmental protection, energy conservation and emission reduction.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows: a honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst, wherein the catalyst active metal component Mn and the interface regulators Cu and M are introduced into the catalyst successively.

[0007] The catalyst has interface characteristics such as lattice distortion and interlayer dislocation, and a large number of boundaries are formed between multivalent metal oxides, which promotes the activation of CO and O2 and inhibits the adsorption of SO2.

[0008] The present invention provides a method for preparing a honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst, comprising the following steps:

[0009] S1: adding KMnO4 solution to divalent manganese salt solution, stirring at room temperature to obtain a reaction precursor, transferring the reaction precursor to an autoclave for hydrothermal reaction, and after the reaction is completed, obtaining a mixed solution, filtering and washing the mixed solution to obtain a precipitate, and drying and calcining the precipitate to obtain Mn monometallic oxide;

[0010] S2: Introducing the precursors of interface regulators Cu and M into Mn monometallic oxide, and obtaining a highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst after drying and calcining;

[0011] S3: Add the binder to the Mn-Cu-M ternary composite metal oxide catalyst, stir evenly to obtain a mud material, age it at room temperature, filter it and extrude it into a shape, dry and calcine it to obtain a honeycomb type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst.

[0012] The concentration of KMnO4 solution is 0.10~0.30mol·L -1 The concentration ratio of the divalent manganese salt solution to the KMnO4 solution is 1:2, and the volume ratio of the two is 1:1; the divalent manganese salt is selected from one of manganese sulfate monohydrate, manganese acetate tetrahydrate, manganese nitrate tetrahydrate and manganese chloride tetrahydrate, preferably manganese sulfate monohydrate.

[0013] The present invention is further configured such that, in step S1, the temperature of the hydrothermal reaction is 100-200°C, the time is 12-24 hours, and the washing standard is pH 7.

[0014] The present invention is further configured such that, in steps S1-S3, the drying temperature is 60-120°C, the time is 6-12 hours, and the calcination temperature is 350-500°C, the time is 2-4 hours.

[0015] The present invention is further configured as follows: in step S2, the method for introducing the interface regulators Cu and M can be a conventional method for loading metals in the catalytic field, selected from one of a coprecipitation method, a deposition precipitation method, an impregnation method, a ball milling method or a direct roasting method; the precipitant of the coprecipitation method is selected from one of sodium carbonate, sodium bicarbonate, potassium carbonate and ammonium oxalate, and the pH regulator is selected from one of sodium hydroxide and potassium hydroxide; the precipitant of the deposition precipitation method is urea.

[0016] The present invention is further configured that, in step S2, the precursor of Cu is a divalent copper salt, selected from one of copper nitrate trihydrate, copper sulfate pentahydrate, copper acetate monohydrate, basic copper carbonate and copper chloride dihydrate, preferably copper nitrate trihydrate; the precursor of M is one of gallium nitrate nonahydrate, indium nitrate nonahydrate, cesium nitrate and ammonium perrhenate;

[0017] The present invention is further configured such that the binder is selected from one of sodium silicate, sodium metaaluminate and sodium aluminosilicate, preferably sodium aluminosilicate.

[0018] The present invention is further configured such that the molar ratio of Mn, Cu and M in the honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst is (4-20):4:1.

[0019] The present invention also provides an application of the above-mentioned honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst for CO oxidation reaction.

[0020] The honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst prepared by the present invention forms a rich interface structure by introducing Mn components, Cu and M components step by step, thereby promoting the adsorption of CO and O2 and inhibiting the adsorption of SO2, thereby greatly improving the catalytic efficiency of CO oxidation and being able to completely convert CO at low temperatures.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The present invention firstly synthesizes a nanorod-shaped Mn monometallic oxide with a tunnel structure by a hydrothermal method, and then further incorporates the interface regulators Cu and M to obtain a honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst. The doping of Cu and M introduces lattice mismatch and distortion, promotes the formation of dislocations and grain boundaries, and these structural defects provide more active sites for the catalytic reaction.

[0023] (2) The present invention optimizes the interfacial properties of the honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst by precisely controlling the molar ratio of Mn, Cu and M, and significantly improves the oxidation activity of the catalyst. The experimental results show that under mild conditions of 89°C, the catalyst can achieve a CO conversion rate of 90%, showing excellent catalytic performance and anti-poisoning properties.

[0024] (3) The honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst of the present invention has a wide range of applications, and is particularly suitable for the purification of flue gas generated by industrial processes such as the steel industry, biomass boilers, and waste incineration power generation boilers. It can not only improve the efficiency of industrial flue gas treatment, but also help reduce energy consumption and pollutant emissions, which is of great significance for promoting the green transformation of industrial production and achieving sustainable development of the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 1 is the XRD diagram of the catalysts prepared in Examples 1, 5, 10 and 13.

[0026] Figure 2 This is the HAADF-STEM image of the catalyst prepared in Example 1.

[0027] Figure 3 and Figure 4 This is the HAADF-STEM image of the catalyst prepared in Example 5.

[0028] Figure 5 It is the H2-TPR diagram of the catalysts prepared in Example 1 and Example 5.

[0029] Figure 6 It is the EPR diagram of the catalyst prepared in Example 1 and Example 5.

[0030] Figure 7 The catalytic performance of the catalysts prepared in Examples 1, 5, 10 and 13 is compared. DETAILED DESCRIPTION

[0031] The technical solution of the present invention is clearly and completely described below through specific embodiments and in conjunction with the accompanying drawings. It should be understood that the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of the present invention.

[0032] The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or conditions recommended by the manufacturers; the raw materials and reagents used are all conventional commercially available products.

[0033] Example 1

[0034] Honeycomb-type highly sulfur-resistant Mn monometallic oxide catalyst MnO x

[0035] Preparation of honeycomb Mn monometallic oxide catalyst MnO by one-step hydrothermal method x , the steps are as follows:

[0036] (1) Dissolve 1.56 g KMnO4 and 0.74 g MnSO4 in 50 mL ultrapure water and disperse by ultrasonic to obtain 0.20 mol·L -1 KMnO4 solution and 0.10 mol·L -1 MnSO4 solution; add 50mL ultrapure water to a 500mL three-necked flask and place it in a 25℃ water bath at a speed of 120r·min -1 The prepared KMnO4 solution and MnSO4 solution were added dropwise under the condition of , and the flow rate was controlled at 1.0 mL min using a constant flow pump. -1 After the feeding was completed, the mixture was stirred vigorously at 25°C for 0.5 h to obtain a brown suspension.

[0037] (2) The brown suspension obtained in step (1) is transferred to a polytetrafluoroethylene hydrothermal reactor, and subjected to a hydrothermal reaction in an oven at 150° C. for 12 h. After the reaction is completed, the mixed solution obtained after the hydrothermal reaction is vacuum filtered and washed multiple times until the pH value is 7 to obtain a black precipitate. The obtained black precipitate is dried in an oven at 80° C. for 4 h, and then calcined in a muffle furnace at 350° C. for 2 h to obtain a highly sulfur-resistant Mn monometallic oxide catalyst.

[0038] (3) 15% of the catalyst mass of sodium aluminosilicate is added to a Mn monometallic oxide catalyst, and an appropriate amount of ultrapure water is added. After being stirred evenly, a slurry is obtained, which is aged at room temperature, filtered, and then extruded and formed. After drying and calcining, a honeycomb-type highly sulfur-resistant Mn monometallic oxide catalyst MnO is obtained. x .

[0039] Example 2

[0040] Honeycomb-type highly sulfur-resistant Mn-Cu-Ga ternary metal oxide catalyst 16 Cu4Ga1O x

[0041] Preparation of honeycomb-type highly sulfur-resistant Mn-Cu-Ga ternary metal oxide catalysts by a two-step hydrothermal-ball milling method 16 Cu4Ga1O x , the steps are as follows:

[0042] (1) Dissolve 1.56 g KMnO4 and 0.74 g MnSO4 in 50 mL ultrapure water and disperse by ultrasonic to obtain 0.20 mol·L -1 KMnO4 solution and 0.10 mol·L -1 MnSO4 solution; add 50mL ultrapure water to a 500mL three-necked flask and place it in a 25℃ water bath at a speed of 120r·min -1 The prepared KMnO4 solution and MnSO4 solution were added dropwise under the condition of , and the flow rate was controlled at 1.0 mL min using a constant flow pump. -1 After the feeding was completed, the mixture was stirred vigorously at 25°C for 0.5 h to obtain a brown suspension.

[0043] (2) The brown suspension obtained in step (1) is transferred to a polytetrafluoroethylene hydrothermal reactor, and subjected to a hydrothermal reaction in an oven at 160° C. for 12 h. After the reaction is completed, the mixed solution obtained after the hydrothermal reaction is vacuum filtered, and washed multiple times until the pH value is 7 to obtain a black precipitate. The obtained black precipitate is dried in an oven at 80° C. for 4 h, and then calcined in a muffle furnace at 360° C. for 2 h to obtain a monometallic Mn oxide.

[0044] (3) Weigh 1.00 g of the Mn metal oxide obtained in step (2), 0.69 g of Cu(NO3)2·3H2O and 0.30 g of Ga(NO3)3·9H2O, add them into a 50 mL zirconia ball mill equipped with 20 zirconia grinding balls with a diameter of 6 mm and a weight of 0.90 g and 6 zirconia grinding balls with a diameter of 10 mm and a weight of 4.15 g, and continuously ball mill them in a ball mill at 400 rpm for 1 hour, i.e., rotate forward for 5 minutes and reverse for 5 minutes for 6 times; the ball milled product is calcined in a muffle furnace at 500°C for 4 hours to obtain a highly sulfur-resistant Mn-Cu-Ga ternary composite metal oxide.

[0045] (4) 15% of the catalyst mass of sodium aluminosilicate is added to a highly sulfur-resistant Mn-Cu-Ga ternary composite metal oxide, and an appropriate amount of ultrapure water is added. After stirring evenly, a slurry is obtained, which is aged at room temperature, filtered, and then extruded and formed. After drying and calcining, a honeycomb-type highly sulfur-resistant Mn-Cu-Ga ternary composite metal oxide is obtained.

[0046] Example 3

[0047] Honeycomb-type highly sulfur-resistant Mn-Cu-In ternary metal oxide catalyst 16 Cu4In1O x

[0048] This embodiment is basically the same as embodiment 2, except that the M precursor added in step (3) is 0.33 g In(NO3)3·9H2O; and Mn is finally obtained. 16 Cu4In1O x catalyst.

[0049] Example 4

[0050] Honeycomb-type highly sulfur-resistant Mn-Cu-Cs ternary metal oxide catalyst 16 Cu4Cs1O x

[0051] This embodiment is basically the same as embodiment 2, except that the M precursor added in step (3) is 0.14 g CsNO3; and finally Mn 16 Cu4Cs1O x catalyst.

[0052] Example 5

[0053] Honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst 16 Cu4Re1O x

[0054] This embodiment is basically the same as embodiment 2, except that the M precursor added in step (3) is 0.19 g NH4ReO4; and finally Mn 16 Cu4Re1O x catalyst.

[0055] Example 6

[0056] Honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst 16 Cu4Re1O x -CP

[0057] This embodiment is basically the same as embodiment 5, except that the method of adding interface modifiers Cu and Re in step (3) is a coprecipitation method; and finally Mn 16 Cu4Re1O x -CP catalyst. The coprecipitation method specifically includes the following steps:

[0058] 0.69 g of Cu(NO3)2·3H2O and 0.19 g of NH4ReO4 were dissolved in 50 mL of ultrapure water and ultrasonically dispersed to obtain an interface regulator solution; 0.70 g of Na2CO3 was dissolved in 50 mL of ultrapure water and ultrasonically dispersed to obtain a precipitant solution; 15.00 g of NaOH was dissolved in 50 mL of ultrapure water and ultrasonically dispersed to obtain a pH regulator solution; 1.00 g of the obtained Mn monometallic oxide was weighed, ultrasonically dispersed in the precipitant solution, transferred to a 500 mL three-necked flask, and placed in a water bath at 25°C at a speed of 120 r·min -1 The interface regulator solution was added dropwise under the condition of , and the flow rate was controlled at 1.0 mL min using a constant flow pump. -1 ; At the same time, a constant flow pump is used to add the pH regulator to control the pH to be constant at 10. After the feeding is completed, continuous and vigorous stirring is continued at 25°C for 1 hour, and then vacuum filtration is performed, and the pH is washed several times until the pH is 7. The mixture is dried in an oven at 120°C for 12 hours, and calcined in a muffle furnace at 500°C for 4 hours for heat treatment to obtain a highly sulfur-resistant Mn-Cu-Re ternary composite metal oxide.

[0059] Example 7

[0060] Honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst 16 Cu4Re1O x -DP

[0061] This embodiment is basically the same as embodiment 5, except that the method of adding interface modifiers Cu and Re in step (3) is a deposition precipitation method; and finally Mn 16 Cu4Re1Ox -DP catalyst. The sedimentation precipitation method specifically includes the following steps:

[0062] 1.00 g of the obtained Mn monometallic oxide, 0.69 g of Cu(NO3)2·3H2O and 0.19 g of NH4ReO4 were weighed, ultrasonically dispersed in 50 mL of ultrapure water, and placed in an oil bath at 90 °C at a speed of 120 r·min. -1 0.10 g of urea was added under the conditions of , and after the feeding was completed, it was continuously and vigorously stirred at 90 ° C for 6 hours, and then vacuum filtered, washed several times until the pH was 7, dried in an oven at 120 ° C for 12 hours, and calcined in a muffle furnace at 500 ° C for 4 hours for heat treatment to obtain a highly sulfur-resistant Mn-Cu-Re ternary composite metal oxide.

[0063] Example 8

[0064] Honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst 16 Cu4Re1O x -IM

[0065] This embodiment is basically the same as embodiment 5, except that the method of adding interface modifiers Cu and Re in step (3) is an equal volume impregnation method; and finally, Mn 16 Cu4Re1O x -IM catalyst. Among them, the equal volume impregnation method specifically includes the following steps:

[0066] Weigh 0.69g Cu(NO3)2·3H2O and 0.19g NH4ReO4 to prepare 1.6mL of interface regulator solution; weigh 1.00g of the obtained Mn monometallic oxide, add the interface regulator solution dropwise thereon and stir thoroughly. After the addition is completed, age at room temperature for 12h, dry in an oven at 120°C for 12h, and calcine in a muffle furnace at 500°C for 4h for heat treatment to obtain a highly sulfur-resistant Mn-Cu-Re ternary composite metal oxide.

[0067] Example 9

[0068] Honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst 16 Cu4Re1O x -C

[0069] This embodiment is basically the same as embodiment 5, except that the method of adding interface modifiers Cu and Re in step (3) is a roasting method; and finally Mn 16 Cu4Re1O x -C catalyst. The calcination method specifically includes the following steps:

[0070] 1.00 g of the obtained Mn monometallic oxide, 0.69 g of Cu(NO3)2·3H2O and 0.19 g of NH4ReO4 were weighed, fully ground, and then calcined in a muffle furnace at 500°C for 4 h for heat treatment to obtain a highly sulfur-resistant Mn-Cu-Re ternary composite metal oxide.

[0071] Example 10

[0072] Honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst 20 Cu4Re1O x

[0073] This embodiment is basically the same as embodiment 5, except that the mass of the Mn metal oxide added in step (3) is 1.25 g; the honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst Mn 20 Cu4Re1O x .

[0074] Embodiment 11

[0075] Honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst 12 Cu4Re1O x

[0076] This embodiment is basically the same as embodiment 5, except that the mass of Mn metal oxide added in step (3) is 0.75 g; the honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst Mn 12 Cu4Re1O x .

[0077] Example 12

[0078] Honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst Mn8Cu4Re1O x

[0079] This embodiment is basically the same as embodiment 5, except that the mass of the Mn metal oxide added in step (3) is 0.50 g; and finally a honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst Mn8Cu4Re1O x .

[0080] Example 13

[0081] Honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst Mn4Cu4Re1O x

[0082] This embodiment is basically the same as embodiment 5, except that the mass of the Mn metal oxide added in step (3) is 0.25 g; and finally a honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst Mn4Cu4Re1O x .

[0083] Embodiment 14

[0084] Honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst 16 Cu4Re1O x -100

[0085] This embodiment is basically the same as embodiment 5, except that the temperature and time of the hydrothermal synthesis in step (2) are 100° C. and 24 h, respectively; and finally a honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst Mn is obtained. 16 Cu4Re1O x -100.

[0086] Embodiment 15

[0087] Honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst 16 Cu4Re1O x -200

[0088] This embodiment is basically the same as embodiment 5, except that the temperature and time of the hydrothermal synthesis in step (2) are 200°C and 12h respectively; and finally a honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst Mn is obtained. 16 Cu4Re1O x -200.

[0089] Example 16

[0090] Honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst 16 Cu4Re1O x -0.1

[0091] This example is basically the same as Example 5, except that in step (1), 0.780 g of KMnO4 was weighed and prepared into 50 mL of 0.10 mol·L -1 KMnO4 solution; weigh 0.370g MnSO4 and prepare 50mL 0.05mol·L -1 MnSO4 solution; finally, a honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst Mn 16 Cu4Re1O x -0.1.

[0092] Embodiment 17

[0093] Honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst 16 Cu4Re1O x -0.3

[0094] This example is basically the same as Example 5, except that in step (1), 2.340 g of KMnO4 was weighed and prepared into 50 mL of 0.30 mol·L -1 KMnO4 solution; weigh 1.110g MnSO4 and prepare 50mL 0.15mol·L -1 MnSO4 solution; finally, a honeycomb-type highly sulfur-resistant Mn-Cu-Re ternary metal oxide catalyst Mn 16 Cu4Re1O x -0.3.

[0095] Comparative Example 1

[0096] Honeycomb Mn monometallic oxide catalyst MnO x -CC

[0097] Preparation of Mn Monometallic Oxide Catalyst MnO by One-step Calcination x -CC, the steps are as follows:

[0098] (1) Weigh 5.00 g of MnCO3 and calcine it in a muffle furnace at 500°C for 4 h to obtain Mn monometallic oxide.

[0099] (2) 15% of the catalyst mass of sodium aluminosilicate is added to Mn monometallic oxide, and an appropriate amount of ultrapure water is added. After being stirred evenly, a slurry is obtained, which is aged at room temperature, filtered, extruded, and dried and calcined to obtain a honeycomb Mn monometallic oxide catalyst MnO x -CC.

[0100] Comparative Example 2

[0101] Honeycomb Mn-Cu-Re ternary composite metal oxide catalyst Mn 16 Cu4Re1O x -CC

[0102] Preparation of Mn-Cu-Re ternary composite metal oxide catalyst by one-step calcination method 16 Cu4Re1O x -CC, the steps are as follows:

[0103] (1) 4.96 g of MnCO3, 0.97 g of Cu2(OH)2CO3 and 0.58 g of NH4ReO4 were weighed, ground and mixed thoroughly, and then calcined in a muffle furnace at 500°C for 4 h to obtain a Mn-Cu-Re ternary composite metal oxide.

[0104] (2) Sodium aluminosilicate with a catalyst weight of 15% was added to Mn-Cu-Re ternary composite metal oxide, and an appropriate amount of ultrapure water was added. After stirring evenly, a slurry was obtained, which was aged at room temperature, filtered, and then extruded and molded. After drying and calcining, a honeycomb Mn-Cu-Re ternary composite metal oxide catalyst Mn was obtained. 16 Cu4Re1O x -CC.

[0105] Comparative Example 3

[0106] Honeycomb Mn-Cu-Re ternary composite metal oxide catalyst Mn 16 Cu4Re1O x -O

[0107] Preparation of Mn-Cu-Re ternary composite metal oxide catalyst by one-step hydrothermal method 16 Cu4Re1O x -O, the steps are as follows:

[0108] (1) 1.56 g KMnO4 was ultrasonically dispersed in 50 mL ultrapure water to obtain 0.20 mol·L -1 KMnO4 solution; 0.74g MnSO4, 0.33g Cu(NO3)2·3H2O and 0.09g NH4ReO4 were ultrasonically dispersed in 50mL ultrapure water to obtain a divalent metal salt solution; 50mL ultrapure water was added to a 500mL three-necked flask, and placed in a 25℃ water bath at a speed of 120r·min -1 The prepared KMnO4 solution and divalent metal salt solution were added dropwise under the condition of , and the flow rate was controlled at 1.0 mL min using a constant flow pump. -1 After the feeding was completed, the mixture was stirred vigorously at 25°C for 0.5 h to obtain a brown suspension.

[0109] (2) transferring the brown suspension obtained in step (1) to a polytetrafluoroethylene hydrothermal reactor and performing a hydrothermal reaction in an oven at 150° C. for 12 h; after the reaction, the resulting mixed solution after the hydrothermal reaction was vacuum filtered and washed multiple times until the pH value was 7 to obtain a black precipitate;

[0110] (3) The black precipitate obtained in step (2) was dried in an oven at 80° C. for 4 h, and then calcined in a muffle furnace at 500° C. for 4 h to obtain a Mn-Cu-Re ternary composite metal oxide.

[0111] (4) Sodium aluminosilicate with a catalyst weight of 15% was added to Mn-Cu-Re ternary composite metal oxide, and an appropriate amount of ultrapure water was added. After stirring evenly, a slurry was obtained, which was aged at room temperature, filtered, and then extruded and formed. After drying and calcining, a honeycomb Mn-Cu-Re ternary composite metal oxide catalyst Mn was obtained. 16 Cu4Re1O x -O.

[0112] Catalyst characterization

[0113] The catalyst prepared above was characterized. Figure 1 1 is the XRD diagram of Example 1, Example 5, Example 10 and Example 13. Figure 1 It can be seen that the highly sulfur-resistant Mn metal oxide catalyst MnO x It has characteristic peaks of manganese dioxide, among which the diffraction peaks at 12.8°, 18.1°, 28.8°, 37.5°, 41.9°, 49.9°, 60.3° and 69.7° correspond to the (110), (200), (310), (211), (301), (411), (521) and (541) crystal planes of the α-MnO2 standard card (JCPDS PDF 44-0141), respectively. The highly sulfur-resistant Mn-Cu-Re ternary composite metal oxide catalyst has characteristic peaks of manganese dioxide and superimposed diffraction peaks of copper oxide, among which the diffraction peaks at 32.5°, 35.5°, 38.7°, 48.7°, 53.5°, 58.3°, 61.5°, 66.3°, 68.1°, 72.4° and 74.8° correspond to the (110), (-111), (111), (-202), (020), (202), (-113), (-311), (220), (311) and (004) crystal planes of the CuO standard card (JCPDS PDF 48-1548), respectively. At the same time, with the increase of the corresponding metal content, the diffraction peaks of the corresponding oxide crystal form gradually appear, and are positively correlated with the metal content. x The peaks at 28.7° and 37.5° of the Mn-Cu-Re ternary composite metal oxide catalyst shift to lower values, indicating that the interface regulators Cu and Re are successfully incorporated into the MnO2 lattice, resulting in lattice distortion and promoting the formation of defect sites. In addition, the highly sulfur-resistant Mn-Cu-Re ternary composite metal oxide catalyst has no obvious diffraction peaks of Re and its oxide, indicating that the Re element is highly dispersed in the catalyst. The crystal form of the composite catalyst of the present invention is good, and no other metal oxides are formed.

[0114] Figure 2The Mn metal oxide catalyst MnO prepared in Example 1 x The HAADF-STEM image shows that the measured lattice spacing is 0.450nm, 0.309nm and 0.215nm, corresponding to the (101), (310) and (301) crystal planes of α-MnO2, respectively. x The catalyst has a rod-like appearance and tunnel structure, and it has highly regular and smooth stripes, and the atomic structure has a good periodic arrangement.

[0115] Figure 3 and Figure 4 The Mn-Cu-Re ternary composite metal oxide catalyst Mn prepared in Example 5 16 Cu4Re1O x In addition to the lattice spacing of α-MnO2, the HAADF-STEM image also measures the lattice spacing of 0.242nm, 0.273nm and 0.295nm, corresponding to the Cu2O(111), CuO(110) and Cu2O(110) crystal planes, respectively. 16 Cu4Re1O x The catalyst has a large number of distorted and blurred lattice fringes, and the incorporation of interface regulators Cu and Re leads to the formation of rich interfaces.

[0116] Figure 5 The MnO prepared in Example 1 x Catalyst and Mn prepared in Example 5 16 Cu4Re1O x H2-TPR diagram of the catalyst. Figure 5 It can be seen that Mn 16 Cu4Re1O x The reduction temperature of the catalyst is lower than that of MnO x The reduction temperature of the catalyst, the incorporation of Cu and Re reduces the reduction temperature, and there is a strong interaction between manganese, copper and rhenium. At the same time, the reduction peak below 200°C in the figure indicates that the surface oxygen species are reduced, indicating the increase of oxygen vacancies.

[0117] Figure 6 The MnO prepared in Example 1 x Catalyst and Mn prepared in Example 5 16 Cu4Re1O x EPR diagram of the catalyst. Figure 6 It can be seen that Mn 16 Cu4Re1O x The oxygen vacancy concentration of the catalyst is higher than that of MnO x The oxygen vacancy concentration of the catalyst and the rich interface formed by the incorporation of Cu and Re promote the generation of oxygen vacancies, which is beneficial to the occurrence of oxidation reactions.

[0118] Example 19: Catalytic performance evaluation

[0119] The catalytic performance and sulfur resistance of the catalysts prepared in Examples 1-17 and Comparative Examples 1-3 in the CO oxidation reaction were evaluated. The CO removal performance evaluation conditions were: reaction temperature of 40-300°C, reaction pressure of normal pressure, and total intake air flow of 250 mL min -1 The raw gas is 0.5% CO, 10% O2, and the rest is N2; the evaluation conditions for sulfur resistance are: reaction temperature is 40-300℃, reaction pressure is normal pressure, and the total inlet flow rate is 250mL·min -1 The raw gas is 0.5% CO, 10% O2, 0.02% SO2, and the rest is N2. The inlet and outlet gases are analyzed by gas chromatography. The catalytic results are shown in Table 1, where T 50 and T 90 The temperatures are when the CO conversion rate is 50% and 90%, respectively. Figure 6 The catalytic performance of the catalysts prepared in Examples 1, 5, 10 and 13 at different temperatures is compared.

[0120] Table 1 Catalytic results of different catalysts in CO oxidation reaction

[0121]

[0122] Comparing Example 1 and Examples 2 to 17 in Table 1, it can be seen that the interface modifiers Cu and M are further doped into the Mn monometallic oxide catalyst MnO x The catalytic performance of the obtained Mn-Cu-M ternary composite metal oxide catalyst is significantly better than that of the Mn single metal oxide catalyst.

[0123] Comparing Examples 2 to 5 in Table 1, it can be seen that the interface modifier Re is superior to Ga, In and Cs. Figure 7 It can be seen that the catalytic performance of the Mn-Cu-Re ternary composite metal oxide catalyst can be further controlled by adjusting the ratio of active Mn species and interface regulators Cu and Re. Among them, the molar ratio of manganese, copper and rhenium is 16:4:1, that is, the catalyst Mn 16 Cu4Re1O x The catalytic performance is the best, and a CO conversion rate of 90% can be achieved under mild conditions of 89°C.

[0124] Comparing Examples 5 to 9 in Table 1, it can be seen that the nanorod-shaped MnO having a tunnel structure is first synthesized by a hydrothermal method. x As a catalyst carrier, Cu and Re were further doped into MnO by ball milling. x The obtained Mn 16 Cu4Re1Ox The catalyst has better catalytic performance.

[0125] By comparing Examples 1 to 17 and Comparative Examples 1 to 3 in Table 1, it can be seen that the catalytic performance and sulfur resistance of the catalysts synthesized by the two-step method (hydrothermal-ball milling method, hydrothermal-coprecipitation method, hydrothermal-sedimentation precipitation method, hydrothermal-equal volume impregnation method and hydrothermal-calcination method) are much better than those of the catalysts synthesized by the one-step method (calcination method and hydrothermal method).

[0126] The present invention adopts the catalyst grain boundary engineering strategy, introduces the active metal component Mn and the interface regulators Cu and M in steps, and constructs a composite metal oxide catalyst with interface characteristics such as lattice distortion and interlayer dislocation. By precisely controlling its interface structure, it can promote the activation of CO and O2 and inhibit the adsorption of SO2, thereby greatly improving the catalytic efficiency of CO oxidation, and efficiently removing CO from the byproduct flue gas of the industrial production process at low temperature, achieving safety, environmental protection, energy saving and emission reduction.

[0127] The above detailed description of the technical solution of the present application is made through specific embodiments, which cannot be used to limit the protection scope of the present application. All equivalent replacements, modifications and modifications made according to the technical concept and spirit of the present application should be included in the protection scope of the present application.

Claims

1. A honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst, characterized in that: The catalyst is obtained by sequentially introducing an active metal component A and an interface regulator B, wherein the active metal component A is Mn, the interface regulator B includes Cu and M, and M is selected from one of Ga, In, Cs and Re.

2. A method for preparing the honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst as claimed in claim 1, characterized in that: The following steps are involved: S1: adding KMnO4 solution to divalent manganese salt solution, stirring at room temperature to obtain a reaction precursor, transferring the reaction precursor to an autoclave for hydrothermal reaction, and after the reaction is completed, obtaining a mixed solution, filtering and washing the mixed solution to obtain a precipitate, and drying and calcining the precipitate to obtain Mn monometallic oxide; S2: Introducing the precursors of interface regulators Cu and M into Mn monometallic oxide, and obtaining a highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst after drying and calcining; S3: Add the binder to the Mn-Cu-M ternary composite metal oxide catalyst, stir evenly to obtain a mud material, age it at room temperature, filter it and extrude it into a shape, dry and calcine it to obtain a honeycomb type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst.

3. The method for preparing the honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst according to claim 2, characterized in that: In step S1, the concentration of KMnO4 solution is 0.10-0.30 mol·L -1 The concentration ratio of the divalent manganese salt solution to the KMnO4 solution is 1:2, and the volume ratio of the two is 1:1; the divalent manganese salt is selected from one of manganese sulfate monohydrate, manganese acetate tetrahydrate, manganese nitrate tetrahydrate and manganese chloride tetrahydrate, preferably manganese sulfate monohydrate.

4. The method for preparing the honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst according to claim 2, characterized in that: In the step S1, the temperature of the hydrothermal reaction is 100-200° C., the time is 12-24 hours, and the washing standard is pH 7.

5. The method for preparing the honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst according to claim 2, characterized in that: In the steps S1-S3, the drying temperature is 60-120° C., the time is 6-12 hours, and the calcination temperature is 350-500° C., the time is 2-4 hours.

6. The method for preparing the honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst according to claim 2, characterized in that: In step S2, the method of introducing the interface regulators Cu and M is selected from one of co-precipitation, deposition precipitation, impregnation, ball milling and direct roasting; the precipitant of the co-precipitation method is selected from one of sodium carbonate, sodium bicarbonate, potassium carbonate and ammonium oxalate, and the pH regulator is selected from one of sodium hydroxide and potassium hydroxide; the precipitant of the deposition precipitation method is urea.

7. The method for preparing the honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst according to claim 2, characterized in that: In step S2, the precursor of Cu is a divalent copper salt, selected from one of copper nitrate trihydrate, copper sulfate pentahydrate, copper acetate monohydrate, basic copper carbonate and copper chloride dihydrate, preferably copper nitrate trihydrate; the precursor of M is one of gallium nitrate nonahydrate, indium nitrate nonahydrate, cesium nitrate and ammonium perrhenate.

8. The method for preparing the honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst according to claim 2, characterized in that: In the step S3, the binder is selected from one of sodium silicate, sodium metaaluminate and sodium aluminosilicate, preferably sodium aluminosilicate.

9. The method for preparing the honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst according to claim 1, characterized in that: The molar ratio of Mn, Cu and M in the honeycomb high sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst is (4-20):4:

1.

10. Application of a catalyst prepared by a method for preparing a honeycomb-type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst, characterized in that: The honeycomb type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst is prepared by the preparation method of the honeycomb type highly sulfur-resistant Mn-Cu-M ternary composite metal oxide catalyst according to any one of claims 2 to 9, and is used for low-temperature removal of CO in flue gas.

Citation Information

Patent Citations

  • Composite catalyst for purifying indoor formaldehyde and preparation method of composite catalyst

    CN102198405A

  • Cu-Ce doped type manganese oxide catalyst, preparation method and application thereof

    CN102513122A

  • Self-support noble metal-modified manganese-based composite oxide catalyst and preparation method and application thereof

    CN108212153A

  • Preparation method of efficient water-resistant copper-doped manganese-based catalyst and application thereof in low-concentration ozone decomposition

    CN109289863A

  • Catalyst for catalyzing oxidization of VOCs as well as preparation method and application of catalyst

    CN110124663A

Cited By

  • Multi-modal intelligent evaluation method for corrosion sensitivity of metal material in deep sea environment

    CN120908076A

  • Deep-sea environment metal material corrosion sensitivity multi-modal intelligent evaluation method

    CN120908076B