Degradable biological phosphate glass and fiber and preparation method thereof
By adopting phosphate bioglass and fibers, the problems of poor bonding and slow degradation of bone repair materials are solved, and bone repair materials with excellent mechanical properties are provided, which can quickly degrade and support bone cell growth and withstand dynamic loads.
Patent Information
- Application Number
- CN202411053582.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing bone repair materials have poor bonding with bone tissue, are prone to loosening or falling off, have slow degradation, hinder the growth of bone cells and are very brittle, and cannot withstand large dynamic loads or impacts.
Phosphate bioglass and fibers are used to prepare degradable phosphate bioglass and fibers by low melting temperature, including specific molar components, and combined with the wire drawing preparation method, biophosphate glass fibers with excellent mechanical properties are prepared.
It achieves a good combination of bone repair materials and bone tissue, rapid degradation does not hinder the growth of bone cells, has good mechanical properties, and can withstand large dynamic loads or impacts. It is an ideal artificial bone repair material.
Smart Images

Figure BDA0004975652570000051
Abstract
Description
Technical Field
[0001] The invention belongs to the field of bone repair, and in particular relates to phosphate bioglass and fiber and a preparation method thereof. Background Art
[0002] Bone repair materials are extremely important tissue engineering regeneration materials, mainly from natural bones and artificial bone repair materials. Repair materials taken from natural bones include autologous bones and allogeneic bones. These materials have limited sources, are prone to cause immune reactions, spread viruses, and transplant surgery can cause donor site damage and transplant site infection. Artificial bone repair materials are widely available and low in price, and can reduce post-transplant immune rejection and infection as well as damage caused by additional surgery. Among them, inert repair materials are mainly metals and alloys, zirconium oxide and other ceramics, which have poor bonding with bone tissue and are easy to loosen or even fall off. Ceramic materials degrade very slowly (Ksp = 2.35×10 -59 ), hindering the growth of bone cells and not conducive to the formation of new bones, and being brittle and unable to withstand large dynamic loads or impacts. The most famous bioglass is 45S5 silicate bioglass, which has a low degradation rate and will hinder the growth of new bone tissue. At the same time, the mechanical properties of composite products prepared from bioglass particles currently used are seriously mismatched with the mechanical properties of human tissue, and composite materials constructed with fibers are needed to assist in adjusting the mechanical properties of the products. Summary of the invention
[0003] In view of the above prior art, the purpose of the present invention is to provide a phosphate bioglass and fiber and a corresponding preparation method. The phosphate glass used in the present invention has a low melting temperature and can be easily made into a melt with good quality, thereby preparing phosphate bioglass fiber.
[0004] The technical solution adopted by the present invention is:
[0005] In a first aspect, the present invention provides a degradable biophosphate glass, wherein the degradable biophosphate glass comprises the following components in molar proportions: P2O5: 40-90%, B2O3: 0-20%, Al2O3: 0-15%, SiO2: 0-15%, Na2O: 0-15%, K2O: 0-15%, CaO: 0-25%, MgO: 0-30%, RO: 6-35%, R2O: 0-25%, P2O5+CaO:>60%;
[0006] The RO is a mixture of MgO, CaO, SrO and BaO, and the R2O is a mixture of Li2O, Na2O, K2O and Rb2O.
[0007] The glass may also contain the following components in molar proportions: P2O5: 40-85%, B2O3: 0-18%, Al2O3: 0-14%, SiO2: 0-14%, Na2O: 0-15%, K2O: 0-15%, CaO: 0-25%, MgO: 0-30%, RO: 6-35%, R2O: 0-25%, P2O5+CaO: >63%.
[0008] The P2O5, Na2O, K2O, CaO, and MgO are introduced by corresponding phosphates or carbonates, and the Al2O3 and SiO2 are introduced by their respective oxides. During preparation, the batch materials are calculated by mass fraction respectively and dried to form agglomerates.
[0009] In a second aspect, the present invention provides a method for preparing the above-mentioned degradable biophosphate glass, comprising the following steps:
[0010] The raw materials for preparing biophosphate glass are mixed evenly and dried, put into a glass melting furnace, heated to 1250-1400°C at a rate of 300-400°C / h, melted for 60-180 minutes, then cooled to 1100-1300°C for homogenization and clarification for 30-60 minutes to obtain glass liquid, and then the glass is taken out and rapidly cooled to prepare degradable biophosphate glass.
[0011] The third aspect of the present invention provides the use of the above-mentioned degradable biophosphate glass in the preparation of biophosphate glass fiber.
[0012] In a fourth aspect, the present invention provides a bio-phosphate glass fiber, wherein the bio-phosphate glass fiber is prepared by drawing in glass liquid based on the preparation of bio-phosphate glass.
[0013] The biophosphate glass fiber comprises the following components in molar proportions: P2O5: 40-90%, B2O3: 0-20%, Al2O3: 0-15%, SiO2: 0-15%, Na2O: 0-15%, K2O: 0-15%, CaO: 0-25%, MgO: 0-30%, TiO2: 0-15%, RO: 6-35%, R2O: 0-25%, P2O5+CaO:>60%;
[0014] The RO is a mixture of MgO, CaO, SrO and BaO, and the R2O is a mixture of Li2O, Na2O, K2O and Rb2O.
[0015] The biophosphate glass fiber may also contain the following components in molar proportions: P2O5: 40-85%, B2O3: 0-18%, Al2O3: 0-14%, SiO2: 0-14%, Na2O: 0-15%, K2O: 0-15%, CaO: 0-25%, MgO: 0-30%, TiO2: 0-14%, RO: 6-35%, R2O: 0-25%, P2O5+CaO:>63%.
[0016] The RO is a mixture of MgO, CaO, SrO and BaO, and the R2O is a mixture of Li2O, Na2O, K2O and Rb2O.
[0017] The P2O5, Na2O, K2O, CaO, MgO, and SrO are introduced by corresponding phosphates or carbonates, introduced by H3BO3, and the remaining P is introduced by phosphoric acid. Al2O3, SiO2, and TiO2 are introduced by their respective oxides. During preparation, the batch materials are calculated by mass fraction respectively and dried to form agglomerates.
[0018] In a fifth aspect, the present invention provides a method for preparing the above-mentioned biophosphate glass fiber, comprising the following steps:
[0019] (1) Preparation of glass liquid: The raw materials for preparing biophosphate glass are mixed uniformly and dried, and then put into a glass melting furnace, heated to 1250-1400° C. at a rate of 300-400° C. / h, melted for 60-180 min, and then cooled to 1100-1300° C. for homogenization and clarification for 30-60 min to obtain glass liquid for preparing fibers;
[0020] (2) Fiber preparation: Drawing from glass liquid at a speed of 1000-2000 m / min to obtain biodegradable biophosphate glass fiber.
[0021] Beneficial effects of the present invention:
[0022] The phosphate bioglass and fiber provided by the present invention and the preparation method thereof can be effectively applied to the field of bone repair, solving the problems of poor bonding between existing repair materials and bone tissue, easy loosening and even falling off. The phosphate bioglass and fiber provided by the present invention degrade quickly, will not hinder the growth of bone cells and are beneficial to the formation of new bones, and have good mechanical properties and can withstand large dynamic loads or impacts, and are ideal artificial bone repair materials. DETAILED DESCRIPTION
[0023] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0024] For ease of understanding of the application, the application will be described more fully below, and preferred embodiments of the application are provided. However, the application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the application more thorough and comprehensive. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the application. The terms used herein in the specification of the application are only for the purpose of describing specific embodiments and are not intended to limit the application. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0025] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amount of ingredients, physicochemical properties, etc. are understood to be adjusted by the term "about" in all cases. For example, therefore, unless otherwise specified, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5 intermediate values.
[0026] Herein, unless otherwise stated, glass compositions are expressed as the mole percent of the amount of a particular component contained therein, calculated as an oxide. Any component having more than one oxidation state may be present in the glass composition in any oxidation state. However, unless otherwise stated, the concentration of such component is expressed as the oxide in which such component is in its lowest oxidation state.
[0027] It should be noted that the term "substantially" may be used herein to represent the inherent degree of uncertainty that may be caused by any quantitative comparison, value, measurement, or other representation. These terms are also used herein to represent that a stated value of a quantity may vary from a stated reference value without resulting in a change in the basic function of the subject matter under consideration. Thus, a glass that is "SiO2-free" or "substantially free of SiO2" is a glass in which SiO2 has not been actively added or dosed into the glass but may be present as a contaminant in very small amounts, (e.g., 500, 400, 300, 200, or 100 parts per million (ppm) or less).
[0028] As mentioned above, the performance of silicate bioglass in current bone repair materials is limited and cannot meet application requirements. During long-term research, technicians found that the use of phosphate bioglass and fiber can solve the problems of poor adhesion to bone tissue, easy loosening or even falling off; extremely slow degradation rate (K sp =2.35×10 -59 ), hindering the growth of bone cells and not conducive to the formation of new bone, and being too brittle to withstand large dynamic loads or impacts.
[0029] Based on this, the present invention provides a phosphate bioglass and fiber and a corresponding preparation method. The phosphate bioglass and fiber and the preparation method provided by the present invention can be effectively applied to the field of bone repair, solving the problems of poor bonding between existing repair materials and bone tissue, easy loosening and even falling off. The phosphate bioglass and fiber provided by the present invention degrade quickly, will not hinder the growth of bone cells, are beneficial to the formation of new bones, and have good mechanical properties and can withstand large dynamic loads or impacts, and are ideal artificial bone repair materials.
[0030] The phosphate bioglass of the present invention contains P2O5 and CaO. In some embodiments, the glass further contains Na2O, K2O, CaO, MgO, Al2O3, and SiO2. In terms of molar percentage, P2O5: 40-85%, B2O3: 0-18%, Al2O3: 0-14%, SiO2: 0-14%, Na2O: 0-15%, K2O: 0-15%, CaO: 0-25%, and MgO: 0-30%. Overall, RO: 6-35%, R2O: 0-25%, P2O5+CaO:>63%, wherein RO is the sum of MgO, CaO, SrO, and BaO, and R2O is the sum of Li2O, Na2O, K2O, and Rb2O.
[0031] The fiber of the phosphate bioglass of the present invention contains P2O5 and CaO. In some embodiments, the glass further contains Na2O, K2O, CaO, MgO, SrO, TiO2, Al2O3, and SiO2. In terms of molar percentage, P2O5: 40-85%, B2O3: 0-18%, Al2O3: 0-14%, SiO2: 0-14%, Na2O: 0-15%, K2O: 0-15%, CaO: 0-25%, MgO: 0-30%, and TiO2: 0-14%. Overall, RO: 6-35%, R2O: 0-25%, and P2O5+CaO:>63%. RO is the sum of MgO, CaO, SrO, and BaO, and R2O is the sum of Li2O, Na2O, K2O, and Rb2O.
[0032] The following detailed description is for illustrative purposes only and is intended to provide further explanation of the present application, rather than to limit the scope of the present invention.
[0033] Example: Preparation of biophosphate glass
[0034] The raw materials of biophosphate glass are weighed, mixed evenly and dried, and put into a glass melting furnace, heated to 1250°C at a rate of 300°C / h, melted for 60 minutes, and then cooled to 1100°C for homogenization and clarification for 30 minutes to obtain glass liquid, and then the glass is taken out and rapidly cooled to prepare degradable biophosphate glass.
[0035] Example: Preparation of Biophosphate Glass Fiber
[0036] The raw materials for preparing biophosphate glass are weighed, mixed evenly and dried, and then put into a glass melting furnace to prepare glass liquid for fiber. Then, the glass liquid is drawn to obtain degradable biophosphate glass fiber. Each embodiment is prepared according to the formula and process conditions in Table 1.
[0037] Table 1: Formula and preparation conditions of phosphate bioglass fibers of various embodiments:
[0038]
[0039] The performance test is performed as follows:
[0040] (1) Fiber diameter: Tested in accordance with the Chinese national standard GB / T 7690.5-2001 Test methods for reinforcing material yarns Part 5: Determination of glass fiber diameter;
[0041] (2) Glass softening point temperature: tested according to ASTM C338-93 (2008) Standard Test Method for Softening Point of Glass;
[0042] (3) Fiber drawing temperature: tested according to ASTM C965-96 (2017) Standard Practice for Measuring Viscosity of Glass Above the Softening Point test standard;
[0043] (4) Glass Bubble Count The number of small bubbles in a glass block was counted under a microscope and divided by the weight to obtain the number of bubbles per unit weight.
[0044] (5) The fiber weight loss rate was calculated by selecting 2 g of fibers of uniform diameter, placing them in 100 ml of human tissue simulation fluid, keeping them at 37 °C for 48 h, then washing and drying them with distilled water, and weighing them with a balance with an accuracy of 0.0001 g.
[0045] The test results show that the biophosphate glass fiber prepared by the present invention has good mechanical properties, excellent tensile strength and elongation at break test results, can withstand large dynamic loads or impacts, and is an ideal artificial bone repair material.
[0046] The degradable phosphate glass fiber prepared by the present invention has the characteristics of low softening point and degradability, and also has excellent fiber spinning formability. The material can be used as a reinforcing material and drug sustained-release carrier for absorbable bone internal fixation composite materials, bone defect repair composite materials, and bone tissue engineering scaffold composite materials, and can also be used as a reinforcing material for degradable environment composite materials, and is an ideal artificial bone repair material.
[0047] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A degradable biophosphate glass, characterized in that: The degradable biophosphate glass comprises the following components in molar proportions: P2O5: 40-90%, B2O3: 0-20%, Al2O3: 0-15%, SiO2: 0-15%, Na2O: 0-15%, K2O: 0-15%, CaO: 0-25%, MgO: 0-30%, RO: 6-35%, R2O: 0-25%, P2O5+CaO:>60%; The RO is a mixture of MgO, CaO, SrO and BaO, and the R2O is a mixture of Li2O, Na2O, K2O and Rb2O.
2. The degradable biophosphate glass according to claim 1, characterized in that: The biophosphate glass may also contain the following components in molar proportions: P2O5: 40-85%, B2O3: 0-18%, Al2O3: 0-14%, SiO2: 0-14%, Na2O: 0-15%, K2O: 0-15%, CaO: 0-25%, MgO: 0-30%, RO: 6-35%, R2O: 0-25%, P2O5+CaO:>63%; The RO is a mixture of MgO, CaO, SrO and BaO, and the R2O is a mixture of Li2O, Na2O, K2O and Rb2O.
3. The degradable biophosphate glass according to claim 1 or 2, characterized in that: The P2O5, Na2O, K2O, CaO, and MgO are introduced by corresponding phosphates or carbonates, introduced by H3BO3, and the remaining P is introduced by phosphoric acid. The Al2O3 and SiO2 are introduced by their respective oxides. During preparation, the batch materials are calculated by mass fraction respectively and dried to form agglomerates.
4. The method for preparing the degradable biophosphate glass according to claim 1 or 2, characterized in that: The method comprises the following steps: mixing raw materials for preparing biophosphate glass uniformly and drying them, putting them into a glass melting furnace, heating them to 1250-1400°C at a speed of 300-400°C / h, melting them for 60-180 minutes, then cooling them to 1100-1300°C, homogenizing and clarifying them for 30-60 minutes to obtain glass liquid, then taking out the glass and rapidly cooling it to prepare degradable biophosphate glass.
5. Use of the degradable biophosphate glass according to claim 1 or 2 in the preparation of biophosphate glass fiber.
6. A biophosphate glass fiber, characterized in that: The bio-phosphate glass fiber is prepared by drawing in glass liquid based on the preparation of the bio-phosphate glass described in claim 1.
7. The biophosphate glass fiber according to claim 6, characterized in that: The biophosphate glass fiber comprises the following components in molar proportions: P2O5: 40-90%, B2O3: 0-20%, Al2O3: 0-15%, SiO2: 0-15%, Na2O: 0-15%, K2O: 0-15%, CaO: 0-25%, MgO: 0-30%, TiO2: 0-15%, RO: 6-35%, R2O: 0-25%, P2O5+CaO:>60%; The RO is a mixture of MgO, CaO, SrO and BaO, and the R2O is a mixture of Li2O, Na2O, K2O and Rb2O.
8. The biophosphate glass fiber according to claim 6, characterized in that: The biophosphate glass fiber may also contain the following components in molar proportions: P2O5: 40-85%, B2O3: 0-18%, Al2O3: 0-14%, SiO2: 0-14%, Na2O: 0-15%, K2O: 0-15%, CaO: 0-25%, MgO: 0-30%, TiO2: 0-14%, RO: 6-35%, R2O: 0-25%, P2O5+CaO:>63%; The RO is a mixture of MgO, CaO, SrO and BaO, and the R2O is a mixture of Li2O, Na2O, K2O and Rb2O.
9. The biophosphate glass fiber according to any one of claims 6 to 8, characterized in that: The P2O5, Na2O, K2O, CaO, MgO, and SrO are introduced by corresponding phosphates or carbonates, introduced by H3BO3, and the remaining P is introduced by phosphoric acid. Al2O3, SiO2, and TiO2 are introduced by their respective oxides. During preparation, the batch materials are calculated by mass fraction respectively and dried to form agglomerates.
10. The method for preparing the biophosphate glass fiber according to any one of claims 6 to 9, characterized in that: The steps include: (1) Preparation of glass liquid: The raw materials for preparing biophosphate glass are mixed uniformly and dried, and then put into a glass melting furnace, heated to 1250-1400° C. at a rate of 300-400° C. / h, melted for 60-180 min, and then cooled to 1100-1300° C. for homogenization and clarification for 30-60 min to obtain glass liquid for preparing fibers; (2) Fiber preparation: Drawing from glass liquid at a speed of 1000-2000 m / min to obtain biodegradable biophosphate glass fiber.
Citation Information
Patent Citations
Biological reactive phosphate based continuous glass fiber textile composite and application thereof
CN105818492A
Bioactive borophosphate glasses
CN109195927A
Bioactive phosphate glasses
CN113227004A
Antimicrobial phosphate glass
US20060172877A1