Rare earth-aluminum organic phosphinate and preparation method, application and composition thereof

By preparing rare earth-aluminum organic phosphinate, the existing smoke problem of aluminum alkyl phosphinate in polymers and the low melting point of zinc diethyl phosphinate are solved, and efficient flame retardant performance and Polymer compatibility improves the temperature resistance of the product.

CN118978549AActive Publication Date: 2024-11-19BAOTOU RESEARCH INSTITUTE OF RARE EARTHS +1

Patent Information

Application Number
CN202411064832.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The existing aluminum alkyl phosphinate is prone to smoke during extrusion or injection molding in polymers with high melting point or high glass transition temperature, which affects product performance, and the melting point of zinc diethyl phosphinate is low, which resists Fuel performance and water resistance need to be improved.

Method used

By using the preparation method of rare earth-aluminum organic phosphinate, the reaction conditions are controlled to obtain rare earth-aluminum organic phosphinate, and the rare earth-aluminum organic phosphinate is improved by adding accelerator and aluminum salt to the mixture of alkyl phosphinate rare earth and water. Temperature resistance and flame retardant properties, and compatibility and fluidity with polymers.

Benefits of technology

Rare earth-aluminum organic phosphinates have good temperature resistance and flame retardant properties, improve the flame retardant properties and compatibility of the polymer, reduce corrosiveness, and show good fluidity in the polymer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978549A_ABST
    Figure CN118978549A_ABST
Patent Text Reader

Abstract

The invention discloses rare earth-aluminum organic phosphinate as well as a preparation method, application and a composition thereof. The preparation method comprises the following steps: adding an accelerant and aluminum salt into a mixed solution of alkyl phosphinic acid rare earth and water to obtain rare earth-aluminum organic phosphinate; wherein the accelerant is a substance capable of generating H < + > in water. The rare earth-aluminum organic phosphinate prepared by the method disclosed by the invention has good temperature resistance and flame retardance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a rare earth-aluminum organic phosphinate and a preparation method, application and composition thereof. Background Art

[0002] Alkyl phosphinates have high thermal stability, high phosphorus content, and excellent flame retardant effect. Commonly used alkyl phosphinate flame retardants include alkyl aluminum phosphinate and alkyl zinc phosphinate. When alkyl aluminum phosphinate is applied to polymers with high melting points or high glass transition temperatures, it will produce smoke during the extrusion or injection molding process, which is harmful to personnel and the environment and affects the performance of the product. Zinc diethylphosphinate has a low melting point.

[0003] CN101475706A discloses an organic phosphonic acid rare earth flame retardant, which is a salt of rare earth elements combined in an organic phosphonic acid structure. The organic phosphonic acid rare earth flame retardant has good temperature resistance, but its water resistance and flame retardancy still need to be improved.

[0004] CN117446767A discloses a method for preparing an infrared radiation composite phase aluminum phosphonate material, comprising preparing an A solution having an Al(NO3)3·9H2O content of 0.1 to 1 mol / L and a B solution having a La(NO3)3·6H2O content of 0.1 to 0.5 mol / L; mixing the A solution and the B solution, controlling the Al 3+ with La 3+ The molar ratio of is 1:(0.1-1) to obtain solution C; add ammonia water to solution C to adjust the pH of the solution to 3-5; then stir at a temperature of 50-100°C for 3-8h to obtain solution D; dissolve potassium phosphate and triethylenetriamine in deionized water and stir thoroughly to obtain solution E; add solution E to solution D, then add polyvinyl alcohol, stir at a temperature of 50-90°C for 2-6h to obtain solution F; freeze-dry solution F and grind to obtain mixture G; heat mixture G to 340-360°C at a rate of 14-16°C / min and keep warm for 1-3h; then heat to 1000-1200°C at a rate of 9-11°C / min, keep warm for 0.8-1.2h, grind to obtain infrared radiation composite phase aluminum phosphate material. The material has a high reflectivity in the infrared range. Summary of the invention

[0005] In view of this, one object of the present invention is to provide a method for preparing a rare earth-aluminum organic phosphinate, and the rare earth-aluminum organic phosphinate prepared by the method of the present invention has good temperature resistance and flame retardant properties. Further, the rare earth-aluminum organic phosphinate of the present invention has good compatibility with polymers and low corrosiveness. Further, the rare earth-aluminum organic phosphinate of the present invention has good fluidity after being added to a polymer. Another object of the present invention is to provide a rare earth-aluminum organic phosphinate. Another object of the present invention is to provide a use of a rare earth-aluminum organic phosphinate. Another object of the present invention is to provide a composition.

[0006] The above purpose is achieved through the following technical solutions.

[0007] In one aspect, the present invention provides a method for preparing a rare earth-aluminum organic phosphinate, comprising the following steps:

[0008] Adding a promoter and an aluminum salt to a mixture of an alkyl phosphinate rare earth and water to obtain a rare earth-aluminum organic phosphinate; wherein the promoter is a + of substance.

[0009] According to the preparation method of the present invention, preferably, the alkyl phosphinate in the alkyl phosphinate rare earth is as shown in formula (I):

[0010]

[0011] wherein R1 and R2 are independently selected from H and C1-C6 alkyl; and R1 and R2 are not H at the same time;

[0012] The accelerator is a water-soluble inorganic acid;

[0013] The aluminum salt is a water-soluble aluminum salt.

[0014] According to the preparation method of the present invention, preferably, the molar ratio of the promoter to the alkyl phosphinate rare earth is 0.2:(3-10), and the molar ratio of the alkyl phosphinate rare earth to the aluminum element in the aluminum salt is (0.4-10):2.

[0015] According to the preparation method of the present invention, preferably, the promoter is used in the form of a promoter aqueous solution, and the promoter aqueous solution is added dropwise to a mixture of alkyl phosphinate rare earth and water;

[0016] The aluminum salt is used in the form of an aluminum salt aqueous solution, which is added dropwise to a mixture of alkyl phosphinate rare earth and water.

[0017] According to the preparation method of the present invention, preferably, after the accelerator and the aluminum salt are added, the reaction is carried out at 50 to 105° C. for 1 to 6 hours.

[0018] The preparation method according to the present invention preferably further comprises the following steps:

[0019] Mixing a first liquid containing water and a rare earth source with a second liquid containing a phosphorus-containing substance and water, and then reacting at 50 to 105° C. to obtain an alkylphosphinate rare earth;

[0020] The rare earth source is selected from one or more of rare earth chlorides, rare earth carbonates, rare earth oxides, rare earth nitrates, rare earth acetates, and rare earth hydroxides;

[0021] The phosphorus-containing substance is selected from one or more of alkyl phosphinate alkali metal salts, alkyl phosphinate ammonium salts, and alkyl phosphonic acid.

[0022] On the other hand, the present invention provides a rare earth-aluminum organic phosphinate, which is obtained by the above preparation method.

[0023] In another aspect, the present invention provides a use of the rare earth-aluminum organic phosphinate in improving the flame retardant properties of polymers.

[0024] In another aspect, the present invention provides a composition comprising the rare earth-aluminum organic phosphinate and an inorganic boron-based flame retardant.

[0025] According to the composition of the present invention, preferably, the composition further comprises a polymer; the polymer is selected from one or more of nylon, polybutylene terephthalate, polyethylene terephthalate, polyurethane, and acrylonitrile-styrene-butadiene copolymer.

[0026] The rare earth-aluminum organic phosphinate prepared by the method of the present invention has good heat resistance and flame retardancy. Furthermore, the rare earth-aluminum organic phosphinate of the present invention has good compatibility with polymers and low corrosivity. Furthermore, the rare earth-aluminum organic phosphinate of the present invention has good fluidity after being added to polymers. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the infrared spectrum of the alkyl phosphinate rare earth obtained in Preparation Example 1.

[0028] Figure 2 This is the infrared spectrum of the alkyl phosphinate rare earth obtained in Preparation Example 2.

[0029] Figure 3 The XRD diagrams are of the rare earth-aluminum organic phosphinates obtained in Examples 1 and 2, and the alkyl phosphinate rare earth obtained in Preparation Example 2.

[0030] Figure 4 This is the XRD diagram of the rare earth-aluminum organic phosphite and aluminum sulfate obtained in Example 1.

[0031] Figure 5 This is the XRD diagram of the rare earth-aluminum organic phosphite and cerium sulfate obtained in Example 1.

[0032] Figure 6 This is the XRD diagram of the rare earth-aluminum organic phosphite and cerium sulfate obtained in Example 2.

[0033] Figure 7 This is the SEM image of the alkyl phosphinate rare earth obtained in Preparation Example 2.

[0034] Figure 8 This is the SEM image of the alkyl phosphinate rare earth obtained in Preparation Example 3.

[0035] Fig. 9 This is the SEM image of the rare earth-aluminum organic phosphinate obtained in Example 1.

[0036] Fig.10 This is the SEM image of the rare earth-aluminum organic phosphinate obtained in Example 2. DETAILED DESCRIPTION

[0037] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0038] <Preparation method of rare earth-aluminum organic phosphinate>

[0039] The preparation method of the rare earth-aluminum organic phosphinate of the present invention comprises the following steps: adding a promoter and an aluminum salt into a mixed solution of alkyl phosphinate rare earth and water to obtain the rare earth-aluminum organic phosphinate.

[0040] The alkyl phosphinate in the alkyl phosphinate rare earth can be represented by formula (I):

[0041]

[0042] In formula (I), R1 and R2 are independently selected from H and C1-C6 alkyl groups; and R1 and R2 are not H at the same time. Preferably, R1 and R2 are independently selected from H and C1-C3 alkyl groups; and R1 and R2 are not H at the same time. More preferably, R1 and R2 are both ethyl groups.

[0043] Examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, neopentyl, n-hexyl, 2-methylpentyl, 3-methylpentyl, 2,3-dimethylbutyl, 2,2-dimethylbutyl.

[0044] According to one embodiment of the present invention, the alkyl phosphinate is diethyl phosphinate.

[0045] The rare earth element in the alkyl phosphite rare earth is selected from one or more of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium. Preferably, the rare earth element in the rare earth phosphite is selected from one or more of lanthanum, cerium and yttrium.

[0046] In the mixed solution of alkyl phosphinate rare earth and water, the mass ratio of alkyl phosphinate rare earth to water may be 1:(1.1-2.2); preferably 1:(1.3-2); more preferably 1:(1.4-1.9).

[0047] The temperature of the mixed solution of the alkyl phosphinate rare earth and water may be 50 to 105°C, preferably 60 to 100°C, and more preferably 70 to 95°C.

[0048] The promoter is capable of generating H + The accelerator may be an inorganic acid. Preferably, it is a water-soluble inorganic acid. Examples of inorganic acids include, but are not limited to, hydrogen chloride, sulfuric acid, acetic acid, and nitric acid. The inorganic acid may be used in the form of its aqueous solution. According to one embodiment of the present invention, the accelerator is hydrochloric acid.

[0049] The accelerator aqueous solution can be added dropwise to the mixture of alkyl phosphinate rare earth and water. The concentration of the accelerator aqueous solution can be 0.5 to 3.5 mol / L, preferably 1 to 3 mol / L, and more preferably 1.5 to 2.5 mol / L.

[0050] The molar ratio of the promoter to the alkyl phosphinate rare earth can be 0.2:(3-10); preferably 0.2:(3.5-9). In certain embodiments, the molar ratio of the promoter to the alkyl phosphinate rare earth is 0.2:(4-5).

[0051] The aluminum salt is preferably an inorganic aluminum salt. Preferably, the aluminum salt is a water-soluble aluminum salt. The aluminum salt can be selected from one or more of aluminum sulfate, aluminum nitrate, aluminum chloride, and aluminum acetate. According to one embodiment of the present invention, the aluminum salt is aluminum sulfate.

[0052] The aluminum salt can be used in the form of an aqueous solution. The aluminum salt aqueous solution can be added dropwise to the mixture of the alkyl phosphinate rare earth and water. The concentration of the aluminum salt aqueous solution can be 10 to 40 wt %, preferably 20 to 35 wt %, and more preferably 25 to 33 wt %.

[0053] The aluminum salt and the promoter are added to the mixture of the alkyl phosphinate rare earth and water respectively. The aluminum salt and the promoter do not contact each other before being added to the mixture. According to one embodiment of the present invention, the promoter is added to the mixture of the alkyl phosphinate rare earth and water, and then the aluminum salt is added.

[0054] The molar ratio of the alkyl phosphinate rare earth to the aluminum element in the aluminum salt can be (0.4-10):2; preferably (0.5-5):2. In some embodiments, the molar ratio of the alkyl phosphinate rare earth to the aluminum element in the aluminum salt is (0.8-1.2):2. In other embodiments, the molar ratio of the alkyl phosphinate rare earth to the aluminum element in the aluminum salt is (1.8-2.2):2.

[0055] The reaction temperature may be 50 to 105°C; preferably 60 to 100°C; more preferably 70 to 95°C.

[0056] The reaction time may be 1 to 6 hours, preferably 2 to 6 hours, and more preferably 3 to 5 hours.

[0057] In some embodiments, the method further comprises the following steps: filtering the reaction product obtained by reacting the mixture of the alkyl phosphinate rare earth and water, the accelerator and the aluminum salt to obtain a solid product. After washing the solid product, drying it at 90 to 150° C., preferably at 100 to 130° C., to obtain a rare earth-aluminum organic phosphinate.

[0058] In some embodiments, the method further comprises the following steps: mixing a first liquid containing water and a rare earth source with a second liquid containing a phosphorus-containing substance and water, and then reacting the mixture at 50-105° C. to obtain an alkyl phosphinate rare earth.

[0059] The rare earth source can be selected from one or more of rare earth chlorides, rare earth carbonates, rare earth oxides, rare earth nitrates, rare earth acetates, and rare earth hydroxides. In some embodiments, the rare earth source is a rare earth carbonate, a rare earth oxide, or a rare earth hydroxide. In other embodiments, the rare earth source is a rare earth chloride, a rare earth nitrate, and a rare earth acetate.

[0060] The rare earth element in the rare earth source is selected from one or more of lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, lutetium, scandium and yttrium. Preferably, the rare earth element is selected from one or more of lanthanum, cerium and yttrium.

[0061] The phosphorus-containing substance can be selected from one or more of alkylphosphinate alkali metal salts, alkylphosphinate ammonium salts, and alkylphosphonic acid. Examples of alkylphosphinate alkali metal salts include, but are not limited to, sodium alkylphosphinate, potassium alkylphosphinate, and lithium alkylphosphinate.

[0062] The alkyl phosphinate contained in the phosphorus-containing substance may be represented by formula (I).

[0063] The alkylphosphonic acid may be represented by formula (II):

[0064]

[0065] In formula (II), R3 and R4 are independently selected from H and C1-C6 alkyl groups; and R3 and R4 are not H at the same time. Preferably, R3 and R4 are independently selected from H and C1-C3 alkyl groups; and R1 and R2 are not H at the same time. More preferably, R3 and R4 are both ethyl groups.

[0066] Examples of alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, neopentyl, n-hexyl, 2-methylpentyl, 3-methylpentyl, 2,3-dimethylbutyl, 2,2-dimethylbutyl.

[0067] According to one embodiment of the present invention, the alkylphosphonic acid is diethylphosphonic acid.

[0068] The reaction temperature may be 60 to 110°C; preferably 70 to 100°C; more preferably 80 to 90°C.

[0069] The reaction time may be 1 to 8 hours, preferably 2 to 6 hours, and more preferably 3 to 4 hours.

[0070] In certain embodiments, the second liquid is added dropwise to the first liquid, thereby mixing the first liquid and the second liquid. The temperature of the first liquid may be 60 to 110°C, preferably 70 to 100°C, and more preferably 80 to 90°C.

[0071] In other embodiments, the first liquid is added dropwise to the second liquid, thereby mixing the first liquid and the second liquid. The temperature of the second liquid may be 60 to 110°C, preferably 70 to 100°C, and more preferably 80 to 90°C.

[0072] The molar ratio of the rare earth element in the rare earth source to the phosphorus-containing substance may be 1:(1-6); preferably 1:(2-5). In certain embodiments, the molar ratio of the rare earth element in the rare earth source to the phosphorus-containing substance is 1:(4-4.5).

[0073] In the first liquid, the mass ratio of the rare earth source to water may be 11:(15-50); preferably 11:(20-40).

[0074] In the second liquid, the mass ratio of the phosphorus-containing substance to water may be 10:(5-95); preferably 10:(10-90).

[0075] In some embodiments, the following steps may be further included: filtering the reaction product obtained by the reaction of the first liquid and the second liquid, and then washing; drying the washed product to obtain the alkyl phosphinate rare earth. The drying temperature may be 90 to 150°C; preferably, 100 to 130°C.

[0076] <Rare earth-aluminum organic phosphinates and their uses>

[0077] The rare earth-aluminum organic phosphinate of the present invention is prepared by the above method. The rare earth-aluminum organic phosphinate can improve the flame retardant properties of polymers. Therefore, the present invention also provides the use of the rare earth-aluminum organic phosphinate in improving the flame retardant properties of polymers.

[0078] The polymer may be selected from one or more of nylon, polybutylene terephthalate, polyethylene terephthalate, polyurethane, and acrylonitrile-styrene-butadiene copolymer. In certain embodiments, the polymer is preferably nylon. Nylon may be selected from one or more of the copolymers of PA6, PA66, PA11, PA12, PA6T, PA6T, and PA66. According to one embodiment of the present invention, nylon is a copolymer of PA6T and PA66.

[0079] <Composition>

[0080] The flame retardant composition of the present invention comprises the above-mentioned rare earth-aluminum-containing organic phosphinate and an inorganic boron flame retardant. The inorganic boron flame retardant can be selected from one or more of borax, boric acid, zinc borate, calcium metaborate, ammonium metaborate, ammonium pentaborate, sodium metaborate, ammonium fluoroborate and zinc fluoroborate. Preferably, the inorganic boron flame retardant is zinc borate. The present invention finds that compounding the above-mentioned rare earth-aluminum-containing organic phosphinate with the inorganic boron flame retardant has a better flame retardant effect.

[0081] The amount of the rare earth-aluminum-containing organic phosphinate may be 5 to 30 parts by weight, preferably 10 to 25 parts by weight, and more preferably 15 to 20 parts by weight.

[0082] The amount of the inorganic boron flame retardant can be 0.3 to 5 parts by weight, preferably 0.5 to 3 parts by weight, and more preferably 1 to 2 parts by weight.

[0083] In certain embodiments, the composition of the present invention further comprises a polymer. The polymer may be selected from one or more of nylon, polybutylene terephthalate, polyethylene terephthalate, polyurethane, acrylonitrile-styrene-butadiene copolymer. In certain embodiments, the polymer is preferably nylon. Nylon may be selected from one or more of the copolymers of PA6, PA66, PA11, PA12, PA6T, PA6T and PA66. According to one embodiment of the present invention, nylon is a copolymer of PA6T and PA66. The amount of the polymer may be 30 to 70 parts by weight; preferably 40 to 60 parts by weight; more preferably 50 to 55 parts by weight.

[0084] The composition of the present invention may further include one or more of an antioxidant, a lubricant, a nucleating agent and glass fibers.

[0085] The amount of the antioxidant used may be 0.1 to 2 parts by weight, preferably 0.2 to 1.5 parts by weight, and more preferably 0.3 to 1 part by weight. The antioxidant may be antioxidant H10.

[0086] The amount of the lubricant can be 0.1 to 1 part by weight, preferably 0.2 to 0.8 part by weight, and more preferably 0.3 to 0.5 part by weight. The lubricant can be wax powder. According to one embodiment of the present invention, the lubricant is AC540A produced by Honeywell.

[0087] The amount of the nucleating agent can be 0.05 to 1 part by weight, preferably 0.1 to 0.5 part by weight, and more preferably 0.2 to 0.3 part by weight. The nucleating agent can be Cav102 produced by Klein.

[0088] The amount of glass fiber used may be 10 to 50 parts by weight, preferably 20 to 40 parts by weight, and more preferably 30 to 35 parts by weight.

[0089] The composition of the present invention can be prepared by the following method: extruding the raw material through a twin-screw extruder to obtain a molding material, cooling the molding material, and then granulating to obtain the composition.

[0090] Here are the raw materials:

[0091] The PA6T / PA66 grade was 1245 and was purchased from Qingdao Sanli Benno New Materials Co., Ltd.

[0092] The glass fiber grade is ECS301UW, which was purchased from Chongqing International Composite Materials Co., Ltd.

[0093] Antioxidant H10, brand is Brüggemann.

[0094] Lubricant AC540A was purchased from Honeywell.

[0095] Nucleating agent Cav102 was purchased from Klein.

[0096] OP-1230, purchased from Klein.

[0097] OP-1240, purchased from Klein.

[0098] Here is the test method:

[0099] If the following test methods require processing into test pieces, the composition shall be dried and then processed into test pieces on an injection molding machine at 280°C, unless otherwise specified.

[0100] UL94: HB grade is evaluated by horizontal burning test, and V0-V2 grade is evaluated by 500W (125mm) vertical burning test.

[0101] Notched impact strength: tested using the method specified in ASTM D256.

[0102] GWIT is measured according to IEC-60695-2-12.

[0103] MVR: MVR at 325°C and 2.16 kg was measured according to the method specified in GB / T 3682.1-2-2018.

[0104] Separation: Place the sample (50 mm × 50 mm × 20 mm) in a constant temperature and humidity chamber, set the temperature to 85°C and the relative humidity to 85%, and visually observe the state of the sample surface after 168 hours.

[0105] Preparation Example 1

[0106] Add 34 parts by weight of water to 11.26 parts by weight of lanthanum cerium carbonate (lanthanum carbonate content is 75wt%, cerium carbonate content is 25wt%), stir evenly and heat to 80°C to obtain a first liquid. Drop a second liquid consisting of 13.39 parts by weight of diethylphosphonic acid and 15 parts by weight of water into the first liquid. After the second liquid is added, react at 80°C for 4h. Filter the reaction product and then wash with water until the pH of the mother liquor is 3-5. Dry the washed solid product to obtain an alkyl phosphinate rare earth.

[0107] Preparation Example 2

[0108] A 33wt% cerium chloride aqueous solution (first liquid) is added dropwise to a 24wt% sodium diethylphosphinate aqueous solution (second liquid) at 80°C. The molar ratio of sodium diethylphosphinate to cerium chloride is 4.5:1. After the addition is completed, the reaction is carried out at 80°C for 4h. The reaction product is filtered and then washed with water. The washed solid product is dried at 120°C to obtain an alkyl phosphinate rare earth.

[0109] Figure 2 The infrared spectrum of the alkylphosphinate rare earth obtained in this preparation example is shown in FIG. 2800-2970 cm -1 The stretching vibration peaks of -CH3 and -CH2- are at 1400~800cm -1 The absorption peaks are those of PO and P=O.

[0110] Preparation Example 3

[0111] A 30wt% yttrium trichloride aqueous solution (first liquid) is added dropwise to a 10wt% sodium diethylphosphinate aqueous solution (second liquid) at a temperature of 80°C. The molar ratio of sodium diethylphosphinate to yttrium trichloride is 3.16:1. After the addition is completed, the reaction is carried out at 80°C for 3h. The reaction product is filtered, and the filter cake is then dried at 125°C to obtain an alkyl phosphinate rare earth.

[0112] Example 1

[0113] 2.12 kg of the alkyl phosphinate rare earth obtained by the method of Preparation Example 2 and 3.0 kg of water were dispersed, stirred and heated to 75°C to obtain a mixed solution. 100 mL of hydrochloric acid with a concentration of 2 mol / L was dripped into the mixed solution, and then an aqueous solution of aluminum sulfate with a concentration of 33 wt% was dripped. The amount of aluminum sulfate used was 1.32 kg. After the aqueous solution of aluminum sulfate was added, the reaction was carried out at 75°C for 5 hours to obtain a reaction product. The reaction product was cooled and filtered to obtain a solid product. The solid product was washed and then dried at 120°C to obtain a rare earth-aluminum organic phosphinate.

[0114] The TG curve shows that the 1wt% thermal weight loss temperature of the rare earth-aluminum organic phosphinate obtained in this example is 338.3°C.

[0115] Depend on Figure 3 It can be seen that the XRD pattern of the product of Example 1 is different from that of Preparation Example 2, and the raw material alkylphosphinate rare earth has reacted. Figure 4 It can be seen that the product of Example 1 does not contain aluminum sulfate (standard card number 30-43). Figure 5 It can be seen that most of the diffraction peaks of the product of Example 1 are inconsistent with the diffraction peaks of cerium sulfate (standard card number 73-1675). The attribution of the diffraction peak around 2θ=10° is similar, which is the diffraction peak of diethylphosphinate cerium salt. This shows that when aluminum sulfate is used, insoluble precipitates of rare earth sulfate will not be generated in the existing reaction system.

[0116] Fig. 9 This is the SEM image of the rare earth-aluminum organic phosphite obtained in Example 1. It can be seen from the image that the product morphology is irregular block or columnar, and some columnar particles have uneven surfaces, proliferated small grains, and small fragment particles attached. Figure 7 This is a SEM image of the alkylphosphinate rare earth obtained in Preparation Example 2, and its microscopic morphology is a rounded rectangular strip crystal with a smooth surface and clear contour lines, which is different from the morphology of the product in Example 1. This indicates that the crystal form has changed after reacting with aluminum sulfate.

[0117] Example 2

[0118] 4.24 kg of the alkyl phosphinate rare earth obtained by the method of Preparation Example 2 and 8.0 kg of water were dispersed, stirred and heated to 95° C. to obtain a mixed solution. 100 mL of hydrochloric acid with a concentration of 2 mol / L was dripped into the mixed solution, and then an aqueous solution of aluminum sulfate with a concentration of 33 wt% was dripped. The amount of aluminum sulfate used was 1.32 kg. After the aqueous solution of aluminum sulfate was added, the reaction was carried out at 95° C. for 4 hours to obtain a reaction product. The reaction product was cooled and filtered to obtain a solid product. The solid product was washed and then dried at 120° C. to obtain a rare earth-aluminum organic phosphinate.

[0119] The TG curve shows that the 1wt% thermal weight loss temperature of the rare earth-aluminum organic phosphinate obtained in this example is 379.7°C.

[0120] Example 3

[0121] Except that the alkyl phosphinate rare earth is obtained by the method of Preparation Example 1, the rest is the same as Example 1.

[0122] Example 4

[0123] Except that the alkyl phosphinate rare earth is obtained by the method of Preparation Example 1, the rest is the same as Example 2.

[0124] Example 5

[0125] The same procedures as in Example 1 were used except that 1.81 kg of the alkyl phosphinate rare earth was obtained by the method of Preparation Example 3.

[0126] Examples 6 to 10 and Comparative Examples 1 to 5

[0127] 53 parts by weight of PA6T / PA66, 0.3 parts by weight of antioxidant H10, 0.5 parts by weight of lubricant AC540C and 0.2 parts by weight of nucleating agent Cav102 were mixed evenly and placed in a twin-screw extruder (model: KTS35 / 44D); the materials shown in Table 1 were mixed and then added to the twin-screw extruder from the first side feed port at 310-330°C; 30 parts by weight of glass fiber were added to the twin-screw extruder through the second side feed port; and the molding material was extruded through the twin-screw extruder to obtain the molding material. The molding material was cooled in a water bath and then granulated to obtain a composition.

[0128] The properties of the composition are shown in Table 1.

[0129] Table 1

[0130]

[0131] Note: Each set of UL94 tests is conducted five times. X*A means that the results of grade A are X times out of five tests.

[0132] Corrosion test

[0133] After PA6T / PA66, antioxidant H10, lubricant AC540C and nucleating agent Cav102 are mixed evenly, they are placed in a twin-screw extruder (model: KTS35 / 44D); a brass block with a mass of m1 is arranged on the die head of the twin-screw extruder; anhydrous zinc borate and a flame retardant (one selected from organic phosphinate, OP-1230, OP-1240) are mixed, and then added to the twin-screw extruder from a first side feed port at 310-330°C; glass fiber is added to the twin-screw extruder through a second side feed port; and the molding material is extruded through the twin-screw extruder to obtain the molding material. The molding material is cooled in a water bath and then granulated.

[0134] The total weight of the raw materials (PA6T / PA66, antioxidant H10, lubricant AC540C, nucleating agent Cav102, anhydrous zinc borate, flame retardant and glass fiber) is 25 kg.

[0135] The mass of the brass block on the die after granulation was measured and recorded as m2. The loss of the brass block was calculated according to the formula (m1-m2) / m1, and the corrosiveness of the composition was judged according to the loss of the brass block.

[0136] The selection and proportion of each raw material are shown in Table 2, and the corrosiveness is shown in Table 2.

[0137] Table 2

[0138]

[0139] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A method for preparing a rare earth-aluminum organic phosphinate, characterized in that: The steps include: Adding a promoter and an aluminum salt to a mixture of an alkyl phosphinate rare earth and water to obtain a rare earth-aluminum organic phosphinate; wherein the promoter is a + of substance.

2. The preparation method according to claim 1, characterized in that: The alkyl phosphinate in the alkyl phosphinate rare earth is as shown in formula (I): wherein R1 and R2 are independently selected from H and C1-C6 alkyl; and R1 and R2 are not H at the same time; The accelerator is a water-soluble inorganic acid; The aluminum salt is a water-soluble aluminum salt.

3. The preparation method according to claim 1, characterized in that: The molar ratio of the promoter to the alkyl phosphinate rare earth is 0.2:(3-10), and the molar ratio of the alkyl phosphinate rare earth to the aluminum element in the aluminum salt is (0.4-10):

2.

4. The preparation method according to claim 1, characterized in that: The promoter is used in the form of a promoter aqueous solution, which is added dropwise to a mixture of alkyl phosphinate rare earth and water; The aluminum salt is used in the form of an aluminum salt aqueous solution, which is added dropwise to a mixture of alkyl phosphinate rare earth and water.

5. The preparation method according to claim 1, characterized in that: After the accelerator and aluminum salt are added, react at 50-105°C for 1-6 hours.

6. The preparation method according to claim 1, characterized in that: The following steps are also included: Mixing a first liquid containing water and a rare earth source with a second liquid containing a phosphorus-containing substance and water, and then reacting at 50 to 105° C. to obtain an alkylphosphinate rare earth; The rare earth source is selected from one or more of rare earth chlorides, rare earth carbonates, rare earth oxides, rare earth nitrates, rare earth acetates, and rare earth hydroxides; The phosphorus-containing substance is selected from one or more of alkyl phosphinate alkali metal salts, alkyl phosphinate ammonium salts, and alkyl phosphonic acid.

7. A rare earth-aluminum organic phosphinate, characterized in that: The rare earth-aluminum organic phosphinate is prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the rare earth-aluminum organic phosphinate according to claim 7 in improving the flame retardant properties of polymers.

9. A composition, characterized in that The composition comprises the rare earth-aluminum organic phosphinate according to claim 7 and an inorganic boron flame retardant.

10. The composition according to claim 9, characterized in that The composition further comprises a polymer; the polymer is selected from one or more of nylon, polybutylene terephthalate, polyethylene terephthalate, polyurethane, and acrylonitrile-styrene-butadiene copolymer.

Citation Information

Patent Citations

  • Organic rare earth metal phosphinate or polymer thereof, and preparation method and application thereof

    CN102850392A

  • Halogen-free solid flame retardant mixture and use thereof

    CN105940085A

  • Halogen-free solid flame retardant mixture and use thereof

    CN109810291A

  • Dialkyl phosphinic acid-aluminum phosphite composite salt and preparation method and application thereof

    CN112876736A

  • Preparation method of metal ion doped metaphosphate near-infrared luminescent material

    CN115746847A

Cited By

  • Flame-retardant anti-aging MPP power cable protection pipe forming process

    CN122381477A