High-strength heat-resistant optical cable and preparation method thereof
By using high-density polyethylene and Si-based composite oxide filler in communication cable sheath material, combined with surface modification treatment, the problem of insufficient protection of the sheath material in high temperature and high stress environments is solved, and higher mechanical strength is achieved and heat resistance, extend the service life of optical cables.
Patent Information
- Application Number
- CN202411028087.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The sheathing material of existing communication optical cables will release toxic gases and thick smoke when burned in natural fires, and the mechanical strength and heat resistance are insufficient, making it difficult to effectively protect the optical fiber signal in high temperature and high stress environments.
Using high-density polyethylene as the matrix, Si-based composite oxide filler is prepared by doping cerium and tantalum, surface hydroxylation and silane reagent treatment are carried out to form acrylamide-acrylic acid copolymer and epoxy groups, and improve the binding of filler and matrix. The heat-resistant sheath layer material is prepared.
It significantly improves the mechanical strength and heat resistance of the sheath layer material, extends the service life of the optical cable in high temperature and high stress environments, and reduces maintenance costs.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of optical cable manufacturing, and in particular to a high-strength heat-resistant optical cable and a preparation method thereof. Background Art
[0002] In recent years, my country's communications industry has developed rapidly, and the demand for optical cables has gradually increased. However, communication optical cables are usually in harsh environments, which can easily cause damage to the metal belt protective layer and distortion of optical fiber signals. In order to improve the reliability and service life of optical fiber signals, they are usually protected with an outer protective layer (sheath material). The outer sheathing material of the optical cable is mainly composed of resins, among which polyethylene (PE) and polyvinyl chloride (PVC) are the most widely used. PVC is cheap and easy to process, and is mostly used in fireproof insulation and sheath flame retardant materials for overhead optical cables. However, when PVC sheath materials burn in natural fires, they will release toxic gases and thick smoke, endangering health and safety. PE has a wide source and relatively superior corrosion resistance, so it has developed rapidly in the insulation and sheath materials of communication optical fiber cables. Summary of the invention
[0003] To this end, the present invention provides a method for preparing a high-strength heat-resistant optical cable, wherein the outer portion of the optical cable is a heat-resistant sheath layer, and the steps of preparing the sheath layer material include:
[0004] (1) preparing a mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol; preparing an aqueous solution of cerium nitrate; preparing an n-butanol solution of tantalum pentachloride; stirring the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol for more than 10 minutes, then adding the aqueous solution of cerium nitrate, the n-butanol solution of tantalum pentachloride and tetraethyl orthosilicate under stirring, continuing to stir for more than 5 minutes after the addition is completed, then adding ammonia water under stirring, heating to 60±5° C. in a water bath after the addition of ammonia water is completed, stirring at this temperature for more than 2 hours, then stirring for 10 to 15 minutes under an ultrasonic environment, separating the solid from the liquid, washing the solid phase with deionized water and ethanol for more than 3 times respectively, then drying at 100° C. for more than 6 hours, and calcining at 550° C. for 3 to 4 hours to obtain a composite powder;
[0005] (2) A Piranha solution is prepared by mixing hydrogen peroxide with a solute mass percentage of 30% and concentrated sulfuric acid with a solute mass percentage of 98% in a volume ratio of hydrogen peroxide: concentrated sulfuric acid = 1:3, and then the composite powder is immersed in the Piranha solution and stirred for 20 to 30 minutes to increase the hydroxyl content on the surface of the powder; then the solid-liquid separation is carried out, the solid phase is washed with deionized water for more than 3 times, and then dried at 70°C for more than 5 hours, the dried solid phase is added to an ethanol aqueous solution, and ultrasonically stirred for more than 10 minutes to form a suspension; then γ-methacryloxypropyltrimethoxysilane is added to the suspension under stirring, and after the addition is completed, the suspension is heated to 75±2°C in a water bath and stirred for more than 3 hours, condensed and refluxed during the insulation process, and the solid-liquid separation is carried out after the insulation is completed, the solid phase is washed with deionized water for more than 3 times, and then dried at 70°C for more than 5 hours, and the dried solid phase Add to white oil, stir ultrasonically for more than 20 minutes to obtain a dispersion, then add a mixed aqueous solution of acrylamide and acrylic acid and N,N'-methylenebisacrylamide to the dispersion under stirring, continue stirring for more than 10 minutes after the addition is completed, then add glacial acetic acid to adjust the pH of the mixture to 6, and stir for more than 20 minutes under ultrasonic environment. After the stirring is completed, the mixture is placed in an argon protection atmosphere, and then ammonium persulfate is added, heated to 70±3° C. in a water bath and stirred for more than 3 hours, solid-liquid separation, the solid phase is washed with deionized water and ethanol for more than 3 times respectively, after washing, it is added to an ethanol solution of glycidoxypropyltrimethoxysilane, stirred for more than 10 minutes under ultrasonic environment to disperse, and then stirred for more than 5 hours, after stirring, solid-liquid separation is completed, the solid phase is washed with ethanol for more than 3 times, and dried at 70° C. for more than 5 hours to obtain a modified powder;
[0006] (3) preparing a composite acetone solution of maleic anhydride and diisopropylbenzene peroxide; uniformly mixing high-density polyethylene particles with glycidyl methacrylate, benzoyl peroxide and xylene in a reactor, then sealing the reactor, filling with nitrogen for protection, heating to 105±3° C. for insulation for more than 2 hours, cooling to room temperature after insulation, opening the reactor, adding the composite acetone solution of maleic anhydride and diisopropylbenzene peroxide to the reactor, and then stirring for more than 20 minutes, sealing the reactor again, filling with nitrogen for protection, heating to 130±3° C. for insulation for more than 1 hour, then cooling to room temperature, opening the reactor, separating the solid from the liquid, washing the solid phase with acetone for more than 3 times, and drying under vacuum at 60° C. to remove the acetone, thereby obtaining a matrix pellet;
[0007] (4) The base pellets, the modified powder, calcium stearate and antioxidant 1010 are mixed uniformly, the mixture is added to an internal mixer and kneaded at 165° C. for more than 10 min, and then transferred to a twin-screw extruder and extruded at 220° C. to obtain the sheath layer material.
[0008] Furthermore, in the step (1), in the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol, the mass ratio of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol is polyethylene glycol octylphenyl ether: ethylene glycol: cyclohexane: n-hexanol = 9-10:1-3:22-25:10; in the aqueous solution of cerium nitrate, the concentration of cerium nitrate is 70-80 g / L, and the solvent is water; in the n-butanol solution of tantalum pentachloride, the concentration of tantalum pentachloride is 10-12 g / L. / L, the solvent is n-butanol; the volume ratio of the mixed solution of polyethylene glycol octyl phenyl ether, ethylene glycol, cyclohexane and n-hexanol and the aqueous solution of cerium nitrate, the n-butanol solution of tantalum pentachloride, tetraethyl orthosilicate and ammonia water is the mixed solution of polyethylene glycol octyl phenyl ether, ethylene glycol, cyclohexane and n-hexanol: aqueous solution of cerium nitrate: n-butanol solution of tantalum pentachloride: tetraethyl orthosilicate: ammonia water = 50: 1-2: 0.8-1.2: 4-5: 7-8, wherein the mass percentage of the solute in the ammonia water is 20%.
[0009] Furthermore, in the step (2), the mass ratio of the composite powder soaked in the Piranha solution is composite powder:Piranha solution=1:100.
[0010] Furthermore, in the step (2), the mass ratio of the dried solid phase added to the ethanol aqueous solution is the dried solid phase: ethanol aqueous solution = 1:50, wherein the volume percentage of ethanol in the ethanol aqueous solution is 90%, and the mass ratio of the added γ-methacryloxypropyltrimethoxysilane to the solid phase in the suspension is γ-methacryloxypropyltrimethoxysilane: solid phase = 2:1.
[0011] Furthermore, in the step (2), the mass ratio of the dried solid phase added to the white oil is solid phase: white oil = 1:50; in the mixed aqueous solution of acrylamide and acrylic acid, the mass percentage of acrylamide is 4%, the mass percentage of acrylic acid is 1%, and the solvent is water; the mass ratio of the mixed aqueous solution of acrylamide and acrylic acid, N,N'-methylenebisacrylamide, and ammonium persulfate added to the dispersion is dispersion: mixed aqueous solution of acrylamide and acrylic acid: N,N'-methylenebisacrylamide: ammonium persulfate = 10:10:0.2-0.3:0.2-0.3.
[0012] Furthermore, in the step (2), the mass percentage of glycidoxypropyltrimethoxysilane in the ethanol solution of glycidoxypropyltrimethoxysilane is 5%, and the mass ratio of the solid phase after washing to the ethanol solution of glycidoxypropyltrimethoxysilane is solid phase: ethanol solution of glycidoxypropyltrimethoxysilane = 1:80.
[0013] Furthermore, in the step (3), in the composite acetone solution of maleic anhydride and dicumyl peroxide, the mass percentage of maleic anhydride is 6% to 8%, the mass percentage of dicumyl peroxide is 0.3% to 0.4%, and the solvent is acetone; the mass ratio of the high-density polyethylene particles to glycidyl methacrylate, benzoyl peroxide, xylene, and the composite acetone solution of maleic anhydride and dicumyl peroxide is high-density polyethylene particles: glycidyl methacrylate: benzoyl peroxide: xylene: composite acetone solution of maleic anhydride and dicumyl peroxide = 1:10:0.3 to 0.4:0.8 to 1:10.
[0014] Furthermore, in the step (4), the mixing mass ratio of the base granules, the modified powder, calcium stearate and the antioxidant 1010 is base granules: modified powder: calcium stearate: antioxidant 1010 = 100: 6-8: 0.7-0.8: 0.7-0.8.
[0015] The beneficial effect of the present invention is that the sheath layer material prepared by the method of the present invention has good mechanical strength and heat resistance, can play a good protective role on the optical cable, so that the service life of the optical cable is extended in the application scene of high temperature and high stress, and the maintenance cost is reduced. The sheath layer material prepared by the present invention is mainly a composite material with high-density polyethylene as the matrix and Si-based composite filler as the reinforcing phase. First, Si-based composite oxide fillers are prepared by doping cerium and tantalum. The role of doping cerium and tantalum is to improve the nucleation rate, refine the particle size of the composite oxide, and significantly increase the specific surface area of the composite oxide, improve the surface energy of the particles, provide preparation for subsequent modification, and can increase the bonding area of the filler and the matrix material, and improve the bonding strength of the two. The subsequent modification is mainly to first perform surface hydroxylation to increase the hydroxyl content of the powder surface; then after being treated with a silane reagent, an acrylamide-acrylic acid copolymer is formed on the surface, and finally epoxy groups are formed on part of the hydroxyl groups by glycidoxypropyltrimethoxysilane to improve the bonding strength of the filler and the high-density polyethylene body, and to avoid the agglomeration of the filler, improve the dispersibility, and thus improve the strength and heat resistance of the composite material. While modifying the filler, high-density polyethylene is also optimized by grafting functional groups to further improve the bonding strength and wettability between the filler and the matrix. DETAILED DESCRIPTION
[0016] The present invention will be further described below in conjunction with the embodiments.
[0017] Example 1
[0018] A method for preparing a high-strength heat-resistant optical cable, wherein the outer portion of the optical cable is a heat-resistant sheath layer, and the steps of preparing the sheath layer material include:
[0019] (1) preparing a mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol; in the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol, the mass ratio of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol is polyethylene glycol octylphenyl ether: ethylene glycol: cyclohexane: n-hexanol = 9:1:22:10; preparing an aqueous solution of cerium nitrate; in the aqueous solution of cerium nitrate, the concentration of cerium nitrate is 70 g / L, and the solvent is water; preparing an n-butanol solution of tantalum pentachloride; in the n-butanol solution of tantalum pentachloride, the concentration of tantalum pentachloride is 10 g / L, and the solvent is n-butanol; stirring the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol for 10 minutes, and then adding the aqueous solution of cerium nitrate, the n-butanol solution of tantalum pentachloride and orthosilicic acid under stirring; tetraethyl orthosilicate, and continue stirring for 5 minutes after the addition is completed, and then add ammonia water under stirring. The volume ratio of the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol and the aqueous solution of cerium nitrate, the n-butanol solution of tantalum pentachloride, tetraethyl orthosilicate and ammonia water is 50:1:0.8:4:7, wherein the mass percentage of the solute in the ammonia water is 20%; after the addition of ammonia water is completed, heat in a water bath to 60±5°C, keep stirring for 2 hours, and then stir for 10 minutes under ultrasonic environment, separate the solid and liquid, wash the solid phase with deionized water and ethanol three times respectively, and then place it under 100°C environment for drying for 6 hours, and calcine at 550°C for 3 hours to obtain a composite powder;
[0020] (2) preparing a Piranha solution by mixing hydrogen peroxide with a solute mass percentage of 30% and concentrated sulfuric acid with a solute mass percentage of 98% in a volume ratio of hydrogen peroxide: concentrated sulfuric acid = 1:3, and then immersing the composite powder in the Piranha solution, wherein the mass ratio of the composite powder immersed in the Piranha solution is composite powder: Piranha solution = 1:100; stirring for 20 minutes to increase the hydroxyl content on the surface of the powder; then separating the solid and the liquid, washing the solid phase with deionized water for 3 times, and then drying at 70°C for 5 hours, adding the dried solid phase to an ethanol aqueous solution, and adding the dried solid phase to the ethanol aqueous solution in a mass ratio of the dried solid phase: ethanol aqueous solution = 1:50, wherein the ethanol water The volume percentage of ethanol in the solution is 90%, and the suspension is formed by stirring for 10 minutes under an ultrasonic environment; then, γ-methacryloxypropyltrimethoxysilane is added to the suspension under stirring, and the mass ratio of the added γ-methacryloxypropyltrimethoxysilane to the solid phase in the suspension is γ-methacryloxypropyltrimethoxysilane: solid phase = 2:1; after the addition is completed, the solution is heated to 75±2° C. in a water bath and kept warm and stirred for 3 hours, condensed and refluxed during the insulation process, and solid-liquid separation is performed after the insulation is completed. The solid phase is washed 3 times with deionized water, and then dried at 70° C. for 5 hours. The dried solid phase is added to white oil, and the mass ratio of the dried solid phase to the white oil is solid phase: white oil = 1:50; stirring for 20 minutes under an ultrasonic environment to obtain a dispersion, Then, a mixed aqueous solution of acrylamide and acrylic acid and N,N'-methylenebisacrylamide are added to the dispersion under stirring. After the addition is completed, stirring is continued for 10 minutes. Then, glacial acetic acid is added to adjust the pH value of the mixture to 6. The mixture is stirred for 20 minutes under an ultrasonic environment. After the stirring is completed, the mixture is placed in an argon protective atmosphere. Then, ammonium persulfate is added. In the mixed aqueous solution of acrylamide and acrylic acid, the mass percentage of acrylamide is 4%, the mass percentage of acrylic acid is 1%, and the solvent is water. The mass ratio of the mixed aqueous solution of acrylamide and acrylic acid, N,N'-methylenebisacrylamide and ammonium persulfate added to the dispersion is dispersion: mixed aqueous solution of acrylamide and acrylic acid: N,N'-methylenebisacrylamide : ammonium persulfate = 10:10:0.2:0.2; heat in a water bath to 70±3°C and keep stirring for 3h, separate the solid and liquid, wash the solid phase with deionized water and ethanol 3 times respectively, add it to the ethanol solution of glycidoxypropyltrimethoxysilane after washing, the mass percentage of glycidoxypropyltrimethoxysilane in the ethanol solution of glycidoxypropyltrimethoxysilane is 5%, and the mass ratio of the solid phase after washing to the ethanol solution of glycidoxypropyltrimethoxysilane is solid phase: ethanol solution of glycidoxypropyltrimethoxysilane = 1:80; stir for 10min to disperse under ultrasonic environment, then stir for 5h, separate the solid and liquid after stirring, wash the solid phase with ethanol 3 times, dry at 70°C for 5h, and obtain modified powder;
[0021] (3) preparing a composite acetone solution of maleic anhydride and diisopropylbenzene peroxide; in the composite acetone solution of maleic anhydride and diisopropylbenzene peroxide, the mass percentage of maleic anhydride is 6%, the mass percentage of diisopropylbenzene peroxide is 0.3%, and the solvent is acetone; in a reaction kettle, high-density polyethylene particles (5000S) are uniformly mixed with glycidyl methacrylate, benzoyl peroxide and xylene, and then the reaction kettle is sealed, filled with nitrogen for protection, and then heated to 105±3°C for 2h. After the insulation is completed, it is cooled to room temperature, the reaction kettle is opened, and the composite acetone solution of maleic anhydride and diisopropylbenzene peroxide is added to the reaction kettle. liquid, the mass ratio of the high-density polyethylene particles to the composite acetone solution of glycidyl methacrylate, benzoyl peroxide, xylene, maleic anhydride and dicumyl peroxide is high-density polyethylene particles: glycidyl methacrylate: benzoyl peroxide: xylene: composite acetone solution of maleic anhydride and dicumyl peroxide = 1:10:0.3:0.8:10; then stirring for 20 minutes, closing the reactor again, filling with nitrogen for protection, heating to 130±3° C. for 1 hour, then cooling to room temperature, opening the reactor, solid-liquid separation, washing the solid phase with acetone for 3 times, and vacuum drying at 60° C. to remove acetone to obtain matrix pellets;
[0022] (4) The base granules, the modified powder, calcium stearate and antioxidant 1010 are uniformly mixed, and the mass ratio of the base granules, the modified powder, calcium stearate and antioxidant 1010 is base granules: modified powder: calcium stearate: antioxidant 1010 = 100:6:0.7:0.7; the mixture is added to an internal mixer and kneaded at 165°C for 10 minutes, and then transferred to a twin-screw extruder and extruded at 220°C to obtain the sheath layer material.
[0023] Example 2
[0024] A method for preparing a high-strength heat-resistant optical cable, wherein the outer portion of the optical cable is a heat-resistant sheath layer, and the steps of preparing the sheath layer material include:
[0025] (1) preparing a mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol; in the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol, the mass ratio of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol is polyethylene glycol octylphenyl ether: ethylene glycol: cyclohexane: n-hexanol = 9:2:23:10; preparing an aqueous solution of cerium nitrate; in the aqueous solution of cerium nitrate, the concentration of cerium nitrate is 70 g / L, and the solvent is water; preparing an n-butanol solution of tantalum pentachloride; in the n-butanol solution of tantalum pentachloride, the concentration of tantalum pentachloride is 11 g / L, and the solvent is n-butanol; stirring the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol for 10 minutes, and then adding the aqueous solution of cerium nitrate, the n-butanol solution of tantalum pentachloride and orthosilicon under stirring; After the addition of the ammonia water is completed, the mixture is heated to 60±5°C in a water bath, stirred for 2h, and then stirred for 10min under an ultrasonic environment, and the solid-liquid separation is performed. The solid phase is washed with deionized water and ethanol for 3 times each, and then dried at 100°C for 6h, and calcined at 550°C for 3h to obtain a composite powder.
[0026] (2) preparing a Piranha solution by mixing hydrogen peroxide with a solute mass percentage of 30% and concentrated sulfuric acid with a solute mass percentage of 98% in a volume ratio of hydrogen peroxide: concentrated sulfuric acid = 1:3, and then immersing the composite powder in the Piranha solution, wherein the mass ratio of the composite powder immersed in the Piranha solution is composite powder: Piranha solution = 1:100; stirring for 20 minutes to increase the hydroxyl content on the surface of the powder; then separating the solid and the liquid, washing the solid phase with deionized water for 3 times, and then drying at 70°C for 5 hours, adding the dried solid phase to an ethanol aqueous solution, and adding the dried solid phase to the ethanol aqueous solution in a mass ratio of the dried solid phase: ethanol aqueous solution = 1:50, wherein the ethanol water The volume percentage of ethanol in the solution is 90%, and the suspension is formed by stirring for 10 minutes under an ultrasonic environment; then, γ-methacryloxypropyltrimethoxysilane is added to the suspension under stirring, and the mass ratio of the added γ-methacryloxypropyltrimethoxysilane to the solid phase in the suspension is γ-methacryloxypropyltrimethoxysilane: solid phase = 2:1; after the addition is completed, the solution is heated to 75±2° C. in a water bath and kept warm and stirred for 3 hours, condensed and refluxed during the insulation process, and solid-liquid separation is performed after the insulation is completed. The solid phase is washed 3 times with deionized water, and then dried at 70° C. for 5 hours. The dried solid phase is added to white oil, and the mass ratio of the dried solid phase to the white oil is solid phase: white oil = 1:50; stirring for 20 minutes under an ultrasonic environment to obtain a dispersion, Then, a mixed aqueous solution of acrylamide and acrylic acid and N,N'-methylenebisacrylamide are added to the dispersion under stirring. After the addition is completed, stirring is continued for 10 minutes. Then, glacial acetic acid is added to adjust the pH value of the mixture to 6. The mixture is stirred for 20 minutes under an ultrasonic environment. After the stirring is completed, the mixture is placed in an argon protective atmosphere. Then, ammonium persulfate is added. In the mixed aqueous solution of acrylamide and acrylic acid, the mass percentage of acrylamide is 4%, the mass percentage of acrylic acid is 1%, and the solvent is water. The mass ratio of the mixed aqueous solution of acrylamide and acrylic acid, N,N'-methylenebisacrylamide and ammonium persulfate added to the dispersion is dispersion: mixed aqueous solution of acrylamide and acrylic acid: N,N'-methylenebisacrylamide : ammonium persulfate = 10:10:0.2:0.2; heat in a water bath to 70±3°C and keep stirring for 3h, separate the solid and liquid, wash the solid phase with deionized water and ethanol 3 times respectively, add it to the ethanol solution of glycidoxypropyltrimethoxysilane after washing, the mass percentage of glycidoxypropyltrimethoxysilane in the ethanol solution of glycidoxypropyltrimethoxysilane is 5%, and the mass ratio of the solid phase after washing to the ethanol solution of glycidoxypropyltrimethoxysilane is solid phase: ethanol solution of glycidoxypropyltrimethoxysilane = 1:80; stir for 10min to disperse under ultrasonic environment, then stir for 5h, separate the solid and liquid after stirring, wash the solid phase with ethanol 3 times, dry at 70°C for 5h, and obtain modified powder;
[0027] (3) preparing a composite acetone solution of maleic anhydride and diisopropylbenzene peroxide; in the composite acetone solution of maleic anhydride and diisopropylbenzene peroxide, the mass percentage of maleic anhydride is 7%, the mass percentage of diisopropylbenzene peroxide is 0.3%, and the solvent is acetone; in a reaction kettle, high-density polyethylene particles (5000S) are uniformly mixed with glycidyl methacrylate, benzoyl peroxide and xylene, and then the reaction kettle is sealed, filled with nitrogen for protection, and then heated to 105±3°C for 2h. After the insulation is completed, it is cooled to room temperature, the reaction kettle is opened, and the composite acetone solution of maleic anhydride and diisopropylbenzene peroxide is added to the reaction kettle. liquid, the mass ratio of the high-density polyethylene particles to the composite acetone solution of glycidyl methacrylate, benzoyl peroxide, xylene, maleic anhydride and dicumyl peroxide is high-density polyethylene particles: glycidyl methacrylate: benzoyl peroxide: xylene: composite acetone solution of maleic anhydride and dicumyl peroxide = 1:10:0.3:0.9:10; then stirring for 20 minutes, closing the reactor again, filling with nitrogen for protection, heating to 130±3° C. for 1 hour, then cooling to room temperature, opening the reactor, solid-liquid separation, washing the solid phase with acetone for 3 times, and vacuum drying at 60° C. to remove acetone to obtain matrix pellets;
[0028] (4) The base granules, the modified powder, calcium stearate and antioxidant 1010 are uniformly mixed, and the mass ratio of the base granules, the modified powder, calcium stearate and antioxidant 1010 is base granules: modified powder: calcium stearate: antioxidant 1010 = 100:7:0.7:0.7; the mixture is added to an internal mixer and kneaded at 165°C for 10 minutes, and then transferred to a twin-screw extruder and extruded at 220°C to obtain the sheath layer material.
[0029] Example 3
[0030] A method for preparing a high-strength heat-resistant optical cable, wherein the outer portion of the optical cable is a heat-resistant sheath layer, and the steps of preparing the sheath layer material include:
[0031] (1) preparing a mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol; in the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol, the mass ratio of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol is polyethylene glycol octylphenyl ether: ethylene glycol: cyclohexane: n-hexanol = 10:2:24:10; preparing an aqueous solution of cerium nitrate; in the aqueous solution of cerium nitrate, the concentration of cerium nitrate is 80 g / L, and the solvent is water; preparing a n-butanol solution of tantalum pentachloride; in the n-butanol solution of tantalum pentachloride, the concentration of tantalum pentachloride is 11 g / L, and the solvent is n-butanol; stirring the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol for 10 minutes, and then adding the aqueous solution of cerium nitrate, the n-butanol solution of tantalum pentachloride and n-butanol solution under stirring; tetraethyl silicate, continue stirring for 5 minutes after the addition is completed, and then add ammonia water under stirring. The volume ratio of the mixed solution of polyethylene glycol octyl phenyl ether, ethylene glycol, cyclohexane and n-hexanol and the aqueous solution of cerium nitrate, the n-butanol solution of tantalum pentachloride, tetraethyl orthosilicate and ammonia water is 50:2:1:5:8: the mixed solution of polyethylene glycol octyl phenyl ether, ethylene glycol, cyclohexane and n-hexanol: the aqueous solution of cerium nitrate: the n-butanol solution of tantalum pentachloride: tetraethyl orthosilicate: ammonia water, wherein the mass percentage of the solute in the ammonia water is 20%; after the addition of ammonia water is completed, heat in a water bath to 60±5°C, keep warm and stir for 2 hours, then stir for 10 minutes under ultrasonic environment, separate solid and liquid, wash the solid phase with deionized water and ethanol three times respectively, then place it under 100°C environment for drying for 6 hours, and calcine at 550°C for 3 hours to obtain a composite powder;
[0032] (2) preparing a Piranha solution by mixing hydrogen peroxide with a solute mass percentage of 30% and concentrated sulfuric acid with a solute mass percentage of 98% in a volume ratio of hydrogen peroxide: concentrated sulfuric acid = 1:3, and then immersing the composite powder in the Piranha solution, wherein the mass ratio of the composite powder immersed in the Piranha solution is composite powder: Piranha solution = 1:100; stirring for 20 minutes to increase the hydroxyl content on the surface of the powder; then separating the solid and the liquid, washing the solid phase with deionized water for 3 times, and then drying at 70°C for 5 hours, adding the dried solid phase to an ethanol aqueous solution, and adding the dried solid phase to the ethanol aqueous solution in a mass ratio of the dried solid phase: ethanol aqueous solution = 1:50, wherein the ethanol water The volume percentage of ethanol in the solution is 90%, and the suspension is formed by stirring for 10 minutes under an ultrasonic environment; then, γ-methacryloxypropyltrimethoxysilane is added to the suspension under stirring, and the mass ratio of the added γ-methacryloxypropyltrimethoxysilane to the solid phase in the suspension is γ-methacryloxypropyltrimethoxysilane: solid phase = 2:1; after the addition is completed, the solution is heated to 75±2° C. in a water bath and kept warm and stirred for 3 hours, condensed and refluxed during the insulation process, and solid-liquid separation is performed after the insulation is completed. The solid phase is washed 3 times with deionized water, and then dried at 70° C. for 5 hours. The dried solid phase is added to white oil, and the mass ratio of the dried solid phase to the white oil is solid phase: white oil = 1:50; stirring for 20 minutes under an ultrasonic environment to obtain a dispersion, Then, a mixed aqueous solution of acrylamide and acrylic acid and N,N'-methylenebisacrylamide are added to the dispersion under stirring. After the addition is completed, stirring is continued for 10 minutes. Then, glacial acetic acid is added to adjust the pH value of the mixture to 6. The mixture is stirred for 20 minutes under an ultrasonic environment. After the stirring is completed, the mixture is placed in an argon protective atmosphere. Then, ammonium persulfate is added. In the mixed aqueous solution of acrylamide and acrylic acid, the mass percentage of acrylamide is 4%, the mass percentage of acrylic acid is 1%, and the solvent is water. The mass ratio of the mixed aqueous solution of acrylamide and acrylic acid, N,N'-methylenebisacrylamide and ammonium persulfate added to the dispersion is dispersion: mixed aqueous solution of acrylamide and acrylic acid: N,N'-methylenebisacrylamide : ammonium persulfate = 10:10:0.3:0.3; heated in a water bath to 70±3°C and stirred for 3h, solid-liquid separation, the solid phase was washed with deionized water and ethanol 3 times respectively, and added to an ethanol solution of glycidoxypropyltrimethoxysilane after washing, the mass percentage of glycidoxypropyltrimethoxysilane in the ethanol solution of glycidoxypropyltrimethoxysilane was 5%, and the mass ratio of the solid phase after washing to the ethanol solution of glycidoxypropyltrimethoxysilane was solid phase: ethanol solution of glycidoxypropyltrimethoxysilane = 1:80; stirred for 10min to disperse under an ultrasonic environment, and then stirred for 5h, solid-liquid separation was performed after stirring, the solid phase was washed 3 times with ethanol, and dried at 70°C for 5h to obtain a modified powder;
[0033] (3) preparing a composite acetone solution of maleic anhydride and diisopropylbenzene peroxide; in the composite acetone solution of maleic anhydride and diisopropylbenzene peroxide, the mass percentage of maleic anhydride is 7%, the mass percentage of diisopropylbenzene peroxide is 0.4%, and the solvent is acetone; in a reaction kettle, high-density polyethylene particles (5000S) are uniformly mixed with glycidyl methacrylate, benzoyl peroxide and xylene, and then the reaction kettle is sealed, filled with nitrogen for protection, and then heated to 105±3°C for 2h. After the insulation is completed, it is cooled to room temperature, the reaction kettle is opened, and the composite acetone solution of maleic anhydride and diisopropylbenzene peroxide is added to the reaction kettle. liquid, the mass ratio of the high-density polyethylene particles to the composite acetone solution of glycidyl methacrylate, benzoyl peroxide, xylene, maleic anhydride and dicumyl peroxide is high-density polyethylene particles: glycidyl methacrylate: benzoyl peroxide: xylene: composite acetone solution of maleic anhydride and dicumyl peroxide = 1:10:0.4:0.9:10; then stirring for 20 minutes, closing the reactor again, filling with nitrogen for protection, heating to 130±3° C. for 1 hour, then cooling to room temperature, opening the reactor, solid-liquid separation, washing the solid phase with acetone for 3 times, and vacuum drying at 60° C. to remove acetone to obtain matrix pellets;
[0034] (4) The base granules, the modified powder, calcium stearate and antioxidant 1010 are uniformly mixed, and the mass ratio of the base granules, the modified powder, calcium stearate and antioxidant 1010 is base granules: modified powder: calcium stearate: antioxidant 1010 = 100:7:0.8:0.8; the mixture is added to an internal mixer and kneaded at 165°C for 10 minutes, and then transferred to a twin-screw extruder and extruded at 220°C to obtain the sheath layer material.
[0035] Example 4
[0036] A method for preparing a high-strength heat-resistant optical cable, wherein the outer portion of the optical cable is a heat-resistant sheath layer, and the steps of preparing the sheath layer material include:
[0037] (1) preparing a mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol; in the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol, the mass ratio of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol is polyethylene glycol octylphenyl ether: ethylene glycol: cyclohexane: n-hexanol = 10:3:25:10; preparing an aqueous solution of cerium nitrate; in the aqueous solution of cerium nitrate, the concentration of cerium nitrate is 80 g / L, and the solvent is water; preparing an n-butanol solution of tantalum pentachloride; in the n-butanol solution of tantalum pentachloride, the concentration of tantalum pentachloride is 12 g / L, and the solvent is n-butanol; stirring the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol for 10 minutes, and then adding the aqueous solution of cerium nitrate, the n-butanol solution of tantalum pentachloride and orthosilicon under stirring; After the addition of the ammonia water is completed, the mixture is heated to 60±5°C in a water bath, stirred for 2h, and then stirred for 10min under an ultrasonic environment, and the solid-liquid separation is performed. The solid phase is washed with deionized water and ethanol for 3 times each, and then dried at 100°C for 6h, and calcined at 550°C for 3h to obtain a composite powder.
[0038] (2) preparing a Piranha solution by mixing hydrogen peroxide with a solute mass percentage of 30% and concentrated sulfuric acid with a solute mass percentage of 98% in a volume ratio of hydrogen peroxide: concentrated sulfuric acid = 1:3, and then immersing the composite powder in the Piranha solution, wherein the mass ratio of the composite powder immersed in the Piranha solution is composite powder: Piranha solution = 1:100; stirring for 20 minutes to increase the hydroxyl content on the surface of the powder; then separating the solid and the liquid, washing the solid phase with deionized water for 3 times, and then drying at 70°C for 5 hours, adding the dried solid phase to an ethanol aqueous solution, and adding the dried solid phase to the ethanol aqueous solution in a mass ratio of the dried solid phase: ethanol aqueous solution = 1:50, wherein the ethanol water The volume percentage of ethanol in the solution is 90%, and the suspension is formed by stirring for 10 minutes under an ultrasonic environment; then, γ-methacryloxypropyltrimethoxysilane is added to the suspension under stirring, and the mass ratio of the added γ-methacryloxypropyltrimethoxysilane to the solid phase in the suspension is γ-methacryloxypropyltrimethoxysilane: solid phase = 2:1; after the addition is completed, the solution is heated to 75±2° C. in a water bath and kept warm and stirred for 3 hours, condensed and refluxed during the insulation process, and solid-liquid separation is performed after the insulation is completed. The solid phase is washed 3 times with deionized water, and then dried at 70° C. for 5 hours. The dried solid phase is added to white oil, and the mass ratio of the dried solid phase to the white oil is solid phase: white oil = 1:50; stirring for 20 minutes under an ultrasonic environment to obtain a dispersion, Then, a mixed aqueous solution of acrylamide and acrylic acid and N,N'-methylenebisacrylamide are added to the dispersion under stirring. After the addition is completed, stirring is continued for 10 minutes. Then, glacial acetic acid is added to adjust the pH value of the mixture to 6. The mixture is stirred for 20 minutes under an ultrasonic environment. After the stirring is completed, the mixture is placed in an argon protective atmosphere. Then, ammonium persulfate is added. In the mixed aqueous solution of acrylamide and acrylic acid, the mass percentage of acrylamide is 4%, the mass percentage of acrylic acid is 1%, and the solvent is water. The mass ratio of the mixed aqueous solution of acrylamide and acrylic acid, N,N'-methylenebisacrylamide and ammonium persulfate added to the dispersion is dispersion: mixed aqueous solution of acrylamide and acrylic acid: N,N'-methylenebisacrylamide : ammonium persulfate = 10:10:0.3:0.3; heated in a water bath to 70±3°C and stirred for 3h, solid-liquid separation, the solid phase was washed with deionized water and ethanol 3 times respectively, and added to an ethanol solution of glycidoxypropyltrimethoxysilane after washing, the mass percentage of glycidoxypropyltrimethoxysilane in the ethanol solution of glycidoxypropyltrimethoxysilane was 5%, and the mass ratio of the solid phase after washing to the ethanol solution of glycidoxypropyltrimethoxysilane was solid phase: ethanol solution of glycidoxypropyltrimethoxysilane = 1:80; stirred for 10min to disperse under an ultrasonic environment, and then stirred for 5h, solid-liquid separation was performed after stirring, the solid phase was washed 3 times with ethanol, and dried at 70°C for 5h to obtain a modified powder;
[0039] (3) preparing a composite acetone solution of maleic anhydride and diisopropylbenzene peroxide; in the composite acetone solution of maleic anhydride and diisopropylbenzene peroxide, the mass percentage of maleic anhydride is 8%, the mass percentage of diisopropylbenzene peroxide is 0.4%, and the solvent is acetone; in a reaction kettle, high-density polyethylene particles (5000S) are uniformly mixed with glycidyl methacrylate, benzoyl peroxide and xylene, and then the reaction kettle is sealed, filled with nitrogen for protection, and then heated to 105±3°C for 2h, cooled to room temperature after the insulation is completed, and the composite acetone solution of maleic anhydride and diisopropylbenzene peroxide is added to the reaction kettle. solution, the mass ratio of the high-density polyethylene particles to the composite acetone solution of glycidyl methacrylate, benzoyl peroxide, xylene, maleic anhydride and dicumyl peroxide is high-density polyethylene particles: glycidyl methacrylate: benzoyl peroxide: xylene: composite acetone solution of maleic anhydride and dicumyl peroxide = 1:10:0.4:1:10; then stirring for 20 minutes, closing the reactor again, filling with nitrogen for protection, heating to 130±3° C. for 1 hour, then cooling to room temperature, opening the reactor, solid-liquid separation, washing the solid phase with acetone for 3 times, and vacuum drying at 60° C. to remove acetone to obtain matrix pellets;
[0040] (4) The base granules, the modified powder, calcium stearate and antioxidant 1010 are uniformly mixed, and the mass ratio of the base granules, the modified powder, calcium stearate and antioxidant 1010 is base granules: modified powder: calcium stearate: antioxidant 1010 = 100:8:0.8:0.8; the mixture is added to an internal mixer and kneaded at 165°C for 10 minutes, and then transferred to a twin-screw extruder and extruded at 220°C to obtain the sheath layer material.
[0041] Comparative Example 1
[0042] A sheath layer material for comparison, the preparation steps of the sheath layer material comprising:
[0043] (1) preparing a mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol; in the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol, the mass ratio of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol is polyethylene glycol octylphenyl ether: ethylene glycol: cyclohexane: n-hexanol = 9:2:23:10; preparing an aqueous solution of cerium nitrate; in the aqueous solution of cerium nitrate, the concentration of cerium nitrate is 70 g / L, and the solvent is water; stirring the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol for 10 minutes, then adding the aqueous solution of cerium nitrate and tetraethyl orthosilicate under stirring, and continuing to stir for 5 minutes after the addition is completed, Then, ammonia water is added under stirring, and the volume ratio of the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol to the aqueous solution of cerium nitrate, tetraethyl orthosilicate and ammonia water is the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol: aqueous solution of cerium nitrate: tetraethyl orthosilicate: ammonia water = 50:1:4:7, wherein the mass percentage of the solute in the ammonia water is 20%; after the addition of ammonia water is completed, the mixture is heated in a water bath to 60±5°C, stirred for 2h, then stirred for 10min under ultrasonic environment, solid-liquid separation is performed, the solid phase is washed with deionized water and ethanol three times respectively, then dried at 100°C for 6h, and calcined at 550°C for 3h to obtain a composite powder;
[0044] (2) preparing a Piranha solution by mixing hydrogen peroxide with a solute mass percentage of 30% and concentrated sulfuric acid with a solute mass percentage of 98% in a volume ratio of hydrogen peroxide: concentrated sulfuric acid = 1:3, and then immersing the composite powder in the Piranha solution, wherein the mass ratio of the composite powder immersed in the Piranha solution is composite powder: Piranha solution = 1:100; stirring for 20 minutes to increase the hydroxyl content on the surface of the powder; then separating the solid and the liquid, washing the solid phase with deionized water for 3 times, and then drying at 70°C for 5 hours, adding the dried solid phase to an ethanol aqueous solution, and adding the dried solid phase to the ethanol aqueous solution in a mass ratio of the dried solid phase: ethanol aqueous solution = 1:50, wherein the ethanol water The volume percentage of ethanol in the solution is 90%, and the suspension is formed by stirring for 10 minutes under an ultrasonic environment; then, γ-methacryloxypropyltrimethoxysilane is added to the suspension under stirring, and the mass ratio of the added γ-methacryloxypropyltrimethoxysilane to the solid phase in the suspension is γ-methacryloxypropyltrimethoxysilane: solid phase = 2:1; after the addition is completed, the solution is heated to 75±2° C. in a water bath and kept warm and stirred for 3 hours, condensed and refluxed during the insulation process, and solid-liquid separation is performed after the insulation is completed. The solid phase is washed 3 times with deionized water, and then dried at 70° C. for 5 hours. The dried solid phase is added to white oil, and the mass ratio of the dried solid phase to the white oil is solid phase: white oil = 1:50; stirring for 20 minutes under an ultrasonic environment to obtain a dispersion, Then, a mixed aqueous solution of acrylamide and acrylic acid and N,N'-methylenebisacrylamide are added to the dispersion under stirring. After the addition is completed, stirring is continued for 10 minutes. Then, glacial acetic acid is added to adjust the pH value of the mixture to 6. The mixture is stirred for 20 minutes under an ultrasonic environment. After the stirring is completed, the mixture is placed in an argon protective atmosphere. Then, ammonium persulfate is added. In the mixed aqueous solution of acrylamide and acrylic acid, the mass percentage of acrylamide is 4%, the mass percentage of acrylic acid is 1%, and the solvent is water. The mass ratio of the mixed aqueous solution of acrylamide and acrylic acid, N,N'-methylenebisacrylamide and ammonium persulfate added to the dispersion is dispersion: mixed aqueous solution of acrylamide and acrylic acid: N,N'-methylenebisacrylamide : ammonium persulfate = 10:10:0.2:0.2; heat in a water bath to 70±3°C and keep stirring for 3h, separate the solid and liquid, wash the solid phase with deionized water and ethanol 3 times respectively, add it to the ethanol solution of glycidoxypropyltrimethoxysilane after washing, the mass percentage of glycidoxypropyltrimethoxysilane in the ethanol solution of glycidoxypropyltrimethoxysilane is 5%, and the mass ratio of the solid phase after washing to the ethanol solution of glycidoxypropyltrimethoxysilane is solid phase: ethanol solution of glycidoxypropyltrimethoxysilane = 1:80; stir for 10min to disperse under ultrasonic environment, then stir for 5h, separate the solid and liquid after stirring, wash the solid phase with ethanol 3 times, dry at 70°C for 5h, and obtain modified powder;
[0045] (3) preparing a composite acetone solution of maleic anhydride and diisopropylbenzene peroxide; in the composite acetone solution of maleic anhydride and diisopropylbenzene peroxide, the mass percentage of maleic anhydride is 7%, the mass percentage of diisopropylbenzene peroxide is 0.3%, and the solvent is acetone; in a reaction kettle, high-density polyethylene particles (5000S) are uniformly mixed with glycidyl methacrylate, benzoyl peroxide and xylene, and then the reaction kettle is sealed, filled with nitrogen for protection, and then heated to 105±3°C for 2h. After the insulation is completed, it is cooled to room temperature, the reaction kettle is opened, and the composite acetone solution of maleic anhydride and diisopropylbenzene peroxide is added to the reaction kettle. liquid, the mass ratio of the high-density polyethylene particles to the composite acetone solution of glycidyl methacrylate, benzoyl peroxide, xylene, maleic anhydride and dicumyl peroxide is high-density polyethylene particles: glycidyl methacrylate: benzoyl peroxide: xylene: composite acetone solution of maleic anhydride and dicumyl peroxide = 1:10:0.3:0.9:10; then stirring for 20 minutes, closing the reactor again, filling with nitrogen for protection, heating to 130±3° C. for 1 hour, then cooling to room temperature, opening the reactor, solid-liquid separation, washing the solid phase with acetone for 3 times, and vacuum drying at 60° C. to remove acetone to obtain matrix pellets;
[0046] (4) The base granules, the modified powder, calcium stearate and antioxidant 1010 are mixed uniformly, and the mass ratio of the base granules, the modified powder, calcium stearate and antioxidant 1010 is base granules: modified powder: calcium stearate: antioxidant 1010 = 100:7:0.7:0.7; the mixture is added to an internal mixer and kneaded at 165°C for 10 minutes, and then transferred to a twin-screw extruder and extruded at 220°C to obtain the sheath layer material described in this comparative example.
[0047] Comparative Example 2
[0048] A sheath layer material for comparison, the preparation steps of the sheath layer material comprising:
[0049] (1) preparing a mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol; in the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol, the mass ratio of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol is polyethylene glycol octylphenyl ether: ethylene glycol: cyclohexane: n-hexanol = 9:2:23:10; preparing an aqueous solution of cerium nitrate; in the aqueous solution of cerium nitrate, the concentration of cerium nitrate is 70 g / L, and the solvent is water; preparing an n-butanol solution of tantalum pentachloride; in the n-butanol solution of tantalum pentachloride, the concentration of tantalum pentachloride is 11 g / L, and the solvent is n-butanol; stirring the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol for 10 minutes, and then adding the aqueous solution of cerium nitrate, the n-butanol solution of tantalum pentachloride and orthosilicon under stirring; After the addition of the ammonia water is completed, the mixture is heated to 60±5°C in a water bath, stirred for 2h, and then stirred for 10min under an ultrasonic environment, and the solid-liquid separation is performed. The solid phase is washed with deionized water and ethanol for 3 times each, and then dried at 100°C for 6h, and calcined at 550°C for 3h to obtain a composite powder.
[0050] (2) preparing a Piranha solution by mixing hydrogen peroxide with a solute mass percentage of 30% and concentrated sulfuric acid with a solute mass percentage of 98% in a volume ratio of hydrogen peroxide: concentrated sulfuric acid = 1:3, and then immersing the composite powder in the Piranha solution, wherein the mass ratio of the composite powder immersed in the Piranha solution is composite powder: Piranha solution = 1:100; stirring for 20 minutes to increase the hydroxyl content on the surface of the powder; then separating the solid and the liquid, washing the solid phase with deionized water for 3 times, and then drying at 70° C. for 5 hours, adding the dried solid phase to an ethanol aqueous solution, wherein the mass ratio of the dried solid phase to the ethanol aqueous solution is the dried solid phase: ethanol aqueous solution = 1:50, wherein the volume percentage of ethanol in the ethanol aqueous solution is 90%, and stirring for 10 minutes under an ultrasonic environment to form a suspension; then adding γ-methacryloxypropyltrimethoxysilane to the suspension under stirring , the mass ratio of γ-methacryloxypropyltrimethoxysilane added to the solid phase in the suspension is γ-methacryloxypropyltrimethoxysilane: solid phase = 2:1; after the addition is completed, the water bath is heated to 75±2°C and stirred for 3 hours, condensed and refluxed during the insulation process, and the solid-liquid separation is completed after the insulation. The solid phase is washed 3 times with deionized water, and then dried at 70°C for 5 hours. The dried solid phase is added to the ethanol solution of glycidoxypropyltrimethoxysilane, and the mass percentage of glycidoxypropyltrimethoxysilane in the ethanol solution of glycidoxypropyltrimethoxysilane is 5%. The mass ratio of the dried solid phase to the ethanol solution of glycidoxypropyltrimethoxysilane is solid phase: ethanol solution of glycidoxypropyltrimethoxysilane = 1:80; stir for 10 minutes to disperse under an ultrasonic environment, and then stir for 5 hours. After stirring, the solid-liquid separation is completed, the solid phase is washed 3 times with ethanol, and dried at 70°C for 5 hours to obtain the modified powder of this comparative example;
[0051] (3) preparing a composite acetone solution of maleic anhydride and diisopropylbenzene peroxide; in the composite acetone solution of maleic anhydride and diisopropylbenzene peroxide, the mass percentage of maleic anhydride is 7%, the mass percentage of diisopropylbenzene peroxide is 0.3%, and the solvent is acetone; in a reaction kettle, high-density polyethylene particles (5000S) are uniformly mixed with glycidyl methacrylate, benzoyl peroxide and xylene, and then the reaction kettle is sealed, filled with nitrogen for protection, and then heated to 105±3°C for 2h. After the insulation is completed, it is cooled to room temperature, the reaction kettle is opened, and the composite acetone solution of maleic anhydride and diisopropylbenzene peroxide is added to the reaction kettle. liquid, the mass ratio of the high-density polyethylene particles to the composite acetone solution of glycidyl methacrylate, benzoyl peroxide, xylene, maleic anhydride and dicumyl peroxide is high-density polyethylene particles: glycidyl methacrylate: benzoyl peroxide: xylene: composite acetone solution of maleic anhydride and dicumyl peroxide = 1:10:0.3:0.9:10; then stirring for 20 minutes, closing the reactor again, filling with nitrogen for protection, heating to 130±3° C. for 1 hour, then cooling to room temperature, opening the reactor, solid-liquid separation, washing the solid phase with acetone for 3 times, and vacuum drying at 60° C. to remove acetone to obtain matrix pellets;
[0052] (4) The base granules, the modified powder, calcium stearate and antioxidant 1010 are mixed uniformly, and the mass ratio of the base granules, the modified powder, calcium stearate and antioxidant 1010 is base granules: modified powder: calcium stearate: antioxidant 1010 = 100:7:0.7:0.7; the mixture is added to an internal mixer and kneaded at 165°C for 10 minutes, and then transferred to a twin-screw extruder and extruded at 220°C to obtain the sheath layer material described in this comparative example.
[0053] Comparative Example 3
[0054] A sheath layer material for comparison, the preparation steps of the sheath layer material comprising:
[0055] (1) preparing a mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol; in the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol, the mass ratio of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol is polyethylene glycol octylphenyl ether: ethylene glycol: cyclohexane: n-hexanol = 9:2:23:10; preparing an aqueous solution of cerium nitrate; in the aqueous solution of cerium nitrate, the concentration of cerium nitrate is 70 g / L, and the solvent is water; preparing an n-butanol solution of tantalum pentachloride; in the n-butanol solution of tantalum pentachloride, the concentration of tantalum pentachloride is 11 g / L, and the solvent is n-butanol; stirring the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol for 10 minutes, and then adding the aqueous solution of cerium nitrate, the n-butanol solution of tantalum pentachloride and orthosilicon under stirring; After the addition of the ammonia water is completed, the mixture is heated to 60±5°C in a water bath, stirred for 2h, and then stirred for 10min under an ultrasonic environment, and the solid-liquid separation is performed. The solid phase is washed with deionized water and ethanol for 3 times each, and then dried at 100°C for 6h, and calcined at 550°C for 3h to obtain a composite powder.
[0056] (2) preparing a Piranha solution by mixing hydrogen peroxide with a solute mass percentage of 30% and concentrated sulfuric acid with a solute mass percentage of 98% in a volume ratio of hydrogen peroxide: concentrated sulfuric acid = 1:3, and then immersing the composite powder in the Piranha solution, wherein the mass ratio of the composite powder immersed in the Piranha solution is composite powder: Piranha solution = 1:100; stirring for 20 minutes to increase the hydroxyl content on the surface of the powder; then separating the solid and the liquid, washing the solid phase with deionized water for 3 times, and then drying at 70°C for 5 hours, adding the dried solid phase to an ethanol aqueous solution, and adding the dried solid phase to the ethanol aqueous solution in a mass ratio of the dried solid phase: ethanol aqueous solution = 1:50, wherein the ethanol water The volume percentage of ethanol in the solution is 90%, and the suspension is formed by stirring for 10 minutes under an ultrasonic environment; then, γ-methacryloxypropyltrimethoxysilane is added to the suspension under stirring, and the mass ratio of the added γ-methacryloxypropyltrimethoxysilane to the solid phase in the suspension is γ-methacryloxypropyltrimethoxysilane: solid phase = 2:1; after the addition is completed, the solution is heated to 75±2° C. in a water bath and kept warm and stirred for 3 hours, condensed and refluxed during the insulation process, and solid-liquid separation is performed after the insulation is completed. The solid phase is washed 3 times with deionized water, and then dried at 70° C. for 5 hours. The dried solid phase is added to white oil, and the mass ratio of the dried solid phase to the white oil is solid phase: white oil = 1:50; stirring for 20 minutes under an ultrasonic environment to obtain a dispersion, Then, a mixed aqueous solution of acrylamide and acrylic acid and N,N'-methylenebisacrylamide are added to the dispersion under stirring. After the addition is completed, stirring is continued for 10 minutes. Then, glacial acetic acid is added to adjust the pH value of the mixture to 6. The mixture is stirred for 20 minutes under an ultrasonic environment. After the stirring is completed, the mixture is placed in an argon protective atmosphere. Then, ammonium persulfate is added. In the mixed aqueous solution of acrylamide and acrylic acid, the mass percentage of acrylamide is 4%, the mass percentage of acrylic acid is 1%, and the solvent is water. The mass ratio of the mixed aqueous solution of acrylamide and acrylic acid, N,N'-methylenebisacrylamide and ammonium persulfate added to the dispersion is dispersion: mixed aqueous solution of acrylamide and acrylic acid: N,N'-methylenebisacrylamide : ammonium persulfate = 10:10:0.2:0.2; heat in a water bath to 70±3°C and keep stirring for 3h, separate the solid and liquid, wash the solid phase with deionized water and ethanol 3 times respectively, add it to the ethanol solution of glycidoxypropyltrimethoxysilane after washing, the mass percentage of glycidoxypropyltrimethoxysilane in the ethanol solution of glycidoxypropyltrimethoxysilane is 5%, and the mass ratio of the solid phase after washing to the ethanol solution of glycidoxypropyltrimethoxysilane is solid phase: ethanol solution of glycidoxypropyltrimethoxysilane = 1:80; stir for 10min to disperse under ultrasonic environment, then stir for 5h, separate the solid and liquid after stirring, wash the solid phase with ethanol 3 times, dry at 70°C for 5h, and obtain modified powder;
[0057] (3) High-density polyethylene pellets (5000S), the modified powder, calcium stearate, and antioxidant 1010 are uniformly mixed, and the mass ratio of the high-density polyethylene pellets, the modified powder, calcium stearate, and antioxidant 1010 is high-density polyethylene pellets: modified powder: calcium stearate: antioxidant 1010 = 100:7:0.7:0.7; the mixture is added to an internal mixer and kneaded at 165°C for 10 minutes, and then transferred to a twin-screw extruder and extruded at 220°C to obtain the sheath layer material described in this comparative example.
[0058] Example 5
[0059] The sheath layer materials prepared by the methods described in the above embodiments and comparative examples were hot-pressed and injection-molded into test specimens at 200°C and 15MPa. The tensile strength of each specimen was tested according to the requirements of standard GB / T1040.1-2018, and the tensile speed was set to 5mm / min. The Vicat softening temperature of each specimen was tested according to the requirements of standard GB / T1633-2000, with a load of 50N and a heating rate of 120°C / h. The results are shown in Table 1.
[0060] As can be seen from Table 1, the sheath layer material prepared by the method of the present invention has good mechanical strength and heat resistance, and can play a good protective role on the optical cable, so that the service life of the optical cable is extended in application scenarios with high temperature and high stress, and the maintenance cost is reduced. The sheath layer material prepared by the present invention is mainly a composite material with high-density polyethylene as the matrix and Si-based composite filler as the reinforcing phase. First, Si-based composite oxide fillers are prepared by doping cerium and tantalum. The role of doping cerium and tantalum is to improve the nucleation rate, refine the particle size of the composite oxide, and significantly increase the specific surface area of the composite oxide, improve the surface energy of the particles, provide preparation for subsequent modification, and increase the bonding area of the filler and the matrix material, and improve the bonding strength of the two. The subsequent modification is mainly to first perform surface hydroxylation to increase the hydroxyl content of the powder surface; then after being treated with a silane reagent, an acrylamide-acrylic acid copolymer is formed on the surface, and finally epoxy groups are formed on some hydroxyls by glycidoxypropyltrimethoxysilane to improve the bonding strength of the filler and the high-density polyethylene body, and to avoid the agglomeration of the filler, improve the dispersibility, and thus improve the strength and heat resistance of the composite material. While modifying the filler, high-density polyethylene is also optimized by grafting functional groups to further improve the bonding strength and wettability between the filler and the matrix.
[0061] Table 1
[0062] Experimental Group Tensile strength(MPa) Vicat softening temperature(℃) Example 1 29.2 86.8 Example 2 30.1 87.7 Example 3 29.8 87.5 Example 4 29.4 87.0 Comparative Example 1 27.5 81.3 Comparative Example 2 25.9 75.4 Comparative Example 3 26.3 79.9
[0063] The technical solution provided by the present invention is introduced in detail above. For those skilled in the art, according to the concept of the embodiments of the present invention, there may be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as limiting the present invention.
Claims
1. A method for preparing a high-strength heat-resistant optical cable, It is characterized in that The outer part of the optical cable is a heat-resistant sheath layer, and the preparation steps of the sheath layer material include: (1) preparing a mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol; preparing an aqueous solution of cerium nitrate; preparing an n-butanol solution of tantalum pentachloride; stirring the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol for more than 10 minutes, then adding the aqueous solution of cerium nitrate, the n-butanol solution of tantalum pentachloride and tetraethyl orthosilicate under stirring, continuing to stir for more than 5 minutes after the addition is completed, then adding ammonia water under stirring, heating to 60±5° C. in a water bath after the addition of ammonia water is completed, stirring at this temperature for more than 2 hours, then stirring for 10 to 15 minutes under an ultrasonic environment, separating the solid from the liquid, washing the solid phase with deionized water and ethanol for more than 3 times respectively, then drying at 100° C. for more than 6 hours, and calcining at 550° C. for 3 to 4 hours to obtain a composite powder; (2) A Piranha solution is prepared by mixing hydrogen peroxide with a solute mass percentage of 30% and concentrated sulfuric acid with a solute mass percentage of 98% in a volume ratio of hydrogen peroxide: concentrated sulfuric acid = 1:3, and then the composite powder is immersed in the Piranha solution and stirred for 20 to 30 minutes to increase the hydroxyl content on the surface of the powder; then the solid-liquid separation is carried out, the solid phase is washed with deionized water for more than 3 times, and then dried at 70°C for more than 5 hours, the dried solid phase is added to an ethanol aqueous solution, and ultrasonically stirred for more than 10 minutes to form a suspension; then γ-methacryloxypropyltrimethoxysilane is added to the suspension under stirring, and after the addition is completed, the suspension is heated to 75±2°C in a water bath and stirred for more than 3 hours, condensed and refluxed during the insulation process, and the solid-liquid separation is carried out after the insulation is completed, the solid phase is washed with deionized water for more than 3 times, and then dried at 70°C for more than 5 hours, and the dried solid phase Add to white oil, stir ultrasonically for more than 20 minutes to obtain a dispersion, then add a mixed aqueous solution of acrylamide and acrylic acid and N,N'-methylenebisacrylamide to the dispersion under stirring, continue stirring for more than 10 minutes after the addition is completed, then add glacial acetic acid to adjust the pH of the mixture to 6, and stir for more than 20 minutes under ultrasonic environment. After the stirring is completed, the mixture is placed in an argon protection atmosphere, and then ammonium persulfate is added, heated to 70±3° C. in a water bath and stirred for more than 3 hours, solid-liquid separation, the solid phase is washed with deionized water and ethanol for more than 3 times respectively, after washing, it is added to an ethanol solution of glycidoxypropyltrimethoxysilane, stirred for more than 10 minutes under ultrasonic environment to disperse, and then stirred for more than 5 hours, after stirring, solid-liquid separation is completed, the solid phase is washed with ethanol for more than 3 times, and dried at 70° C. for more than 5 hours to obtain a modified powder; (3) preparing a composite acetone solution of maleic anhydride and diisopropylbenzene peroxide; uniformly mixing high-density polyethylene particles with glycidyl methacrylate, benzoyl peroxide and xylene in a reactor, then sealing the reactor, filling with nitrogen for protection, heating to 105±3° C. for insulation for more than 2 hours, cooling to room temperature after insulation, opening the reactor, adding the composite acetone solution of maleic anhydride and diisopropylbenzene peroxide to the reactor, and then stirring for more than 20 minutes, sealing the reactor again, filling with nitrogen for protection, heating to 130±3° C. for insulation for more than 1 hour, then cooling to room temperature, opening the reactor, separating the solid from the liquid, washing the solid phase with acetone for more than 3 times, and drying under vacuum at 60° C. to remove the acetone, thereby obtaining a matrix pellet; (4) The base pellets, the modified powder, calcium stearate and antioxidant 1010 are mixed uniformly, the mixture is added to an internal mixer and kneaded at 165° C. for more than 10 min, and then transferred to a twin-screw extruder and extruded at 220° C. to obtain the sheath layer material.
2. A method for preparing a high-strength heat-resistant optical cable according to claim 1, It is characterized in that In the step (1), in the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol, the mass ratio of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol is polyethylene glycol octylphenyl ether: ethylene glycol: cyclohexane: n-hexanol = 9-10:1-3:22-25:10; in the aqueous solution of cerium nitrate, the concentration of cerium nitrate is 70-80 g / L, and the solvent is water; in the n-butanol solution of tantalum pentachloride, the concentration of tantalum pentachloride is 10-12 g / L , the solvent is n-butanol; the volume ratio of the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol and the aqueous solution of cerium nitrate, the n-butanol solution of tantalum pentachloride, tetraethyl orthosilicate and ammonia water is the mixed solution of polyethylene glycol octylphenyl ether, ethylene glycol, cyclohexane and n-hexanol: aqueous solution of cerium nitrate: n-butanol solution of tantalum pentachloride: tetraethyl orthosilicate: ammonia water = 50: 1-2: 0.8-1.2: 4-5: 7-8, wherein the mass percentage of the solute in the ammonia water is 20%.
3. A method for preparing a high-strength heat-resistant optical cable according to claim 1, It is characterized in that In the step (2), the mass ratio of the composite powder soaked in the Piranha solution is composite powder:Piranha solution=1:
100.
4. A method for preparing a high-strength heat-resistant optical cable according to claim 1, It is characterized in that In the step (2), the mass ratio of the dried solid phase added to the ethanol aqueous solution is the dried solid phase: ethanol aqueous solution = 1:50, wherein the volume percentage of ethanol in the ethanol aqueous solution is 90%, and the mass ratio of the added γ-methacryloxypropyltrimethoxysilane to the solid phase in the suspension is γ-methacryloxypropyltrimethoxysilane: solid phase = 2:
1.
5. A method for preparing a high-strength heat-resistant optical cable according to claim 1, It is characterized in that In the step (2), the mass ratio of the dried solid phase added to the white oil is solid phase: white oil = 1:50; in the mixed aqueous solution of acrylamide and acrylic acid, the mass percentage of acrylamide is 4%, the mass percentage of acrylic acid is 1%, and the solvent is water; the mass ratio of the mixed aqueous solution of acrylamide and acrylic acid, N,N'-methylenebisacrylamide, and ammonium persulfate added to the dispersion is dispersion: mixed aqueous solution of acrylamide and acrylic acid: N,N'-methylenebisacrylamide: ammonium persulfate = 10:10:0.2-0.3:0.2-0.
3.
6. A method for preparing a high-strength heat-resistant optical cable according to claim 1, It is characterized in that In the step (2), the mass percentage of glycidoxypropyltrimethoxysilane in the ethanol solution of glycidoxypropyltrimethoxysilane is 5%, and the mass ratio of the solid phase after washing to the ethanol solution of glycidoxypropyltrimethoxysilane is solid phase: ethanol solution of glycidoxypropyltrimethoxysilane = 1:
80.
7. A method for preparing a high-strength heat-resistant optical cable according to claim 1, It is characterized in that In the step (3), in the composite acetone solution of maleic anhydride and dicumyl peroxide, the mass percentage of maleic anhydride is 6% to 8%, the mass percentage of dicumyl peroxide is 0.3% to 0.4%, and the solvent is acetone; the mass ratio of the high-density polyethylene particles to glycidyl methacrylate, benzoyl peroxide, xylene, and the composite acetone solution of maleic anhydride and dicumyl peroxide is high-density polyethylene particles: glycidyl methacrylate: benzoyl peroxide: xylene: composite acetone solution of maleic anhydride and dicumyl peroxide = 1:10:0.3 to 0.4:0.8 to 1:
10.
8. A method for preparing a high-strength heat-resistant optical cable according to claim 1, It is characterized in that In the step (4), the mixing mass ratio of the base granules, the modified powder, calcium stearate and the antioxidant 1010 is base granules: modified powder: calcium stearate: antioxidant 1010 = 100: 6-8: 0.7-0.8: 0.7-0.8.