Thin film transistor and preparation method thereof
By adopting a three-layer structure of zinc, aluminum, tungsten oxide layer and silver layer in thin film transistors, combining alumina and tungsten elements, the problem of high surface resistance and Schottky contact of traditional transparent oxide electrodes is solved, and the bending stress stability is improved and electrical properties enhance the visible light transmittance and mobility of thin film transistors.
Patent Information
- Application Number
- CN202411050253.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
The existing transparent oxide electrode has a high surface resistance during low temperature preparation, resulting in delayed RC information contact with Schottky, deteriorating the gate voltage modulation effect of thin film transistors, and poor bending stress stability.
The first zinc-aluminum-tungsten oxide layer, a silver layer, and a second zinc-aluminum-tungsten oxide layer are formed on the flexible substrate as the source and drain electrodes by using the co-sputtering method and the radio frequency magnetron sputtering method, and the first zinc-aluminum-tungsten oxide layer, a silver layer and a second zinc-aluminum-tungsten oxide layer are formed as the source and drain electrodes on the flexible substrate, and the first zinc-aluminum-tungsten oxide layer is formed as the source and drain electrodes, through the zinc oxide. Add alumina and tungsten elements to form a stable amorphous structure and ohmic contact, reduce oxygen vacancy, and improve electrical properties.
The bending stress stability and electrical properties of the source and drain electrodes are improved, the resistance is reduced, the visible light transmittance and mobility of thin film transistors are enhanced, and the stability is improved.
Smart Images

Figure CN118983225A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of semiconductor devices, and in particular to a thin film transistor and a method for preparing the same. Background Art
[0002] As an important switching component, thin film transistor is one of the most widely used devices in driving circuits. With the continuous development of science and technology, the requirements for the flexibility and transparency of thin film transistors are becoming higher and higher, forming transparent and rollable thin film transistors. The components of transparent and rollable thin film transistors, including the materials of electrodes, substrates, channel layers and dielectric layers, can simultaneously meet the requirements of visible light transmittance and rollability. Among them, the electrodes include source electrodes, drain electrodes and gate electrodes.
[0003] In the prior art, the specific materials of the electrodes are mainly traditional transparent oxides, such as aluminum-doped zinc oxide, gallium-doped zinc oxide, indium tin oxide, etc. However, when the traditional transparent oxides are prepared at low temperatures, they have higher surface resistance than metal electrodes, which makes it easy to produce RC information delay when the traditional transparent oxides are used as source or drain electrodes. On the other hand, since Schottky contact is easily formed between them and the channel layer, the gate voltage modulation effect of the transparent rollable thin film transistor is deteriorated. In addition, the source electrode and the drain electrode in the prior art also have microscopic defects formed inside after multiple bending, which deteriorates the electrical performance of the electrode, that is, the bending stress stability is poor, thereby making the bending stress stability of the thin film transistor poor. Summary of the invention
[0004] The purpose of the present application is to provide a thin film transistor and a method for preparing the same, which can improve the bending stress stability and electrical performance of the source and drain.
[0005] On the one hand, an embodiment of the present application provides a method for preparing a thin film transistor, including providing a flexible substrate and forming a channel layer on the flexible substrate; forming a first zinc aluminum tungsten oxide layer, a silver layer, and a second zinc aluminum tungsten oxide layer in the same layer and material on the channel layer as a source and a drain; forming a dielectric layer on the channel layer with the source and the drain, the dielectric layer being located between the source and the drain; and forming a gate on the dielectric layer.
[0006] As an practicable method, a first zinc-aluminum-tungsten oxide layer, a silver layer, and a second zinc-aluminum-tungsten oxide layer are sequentially formed on the channel layer with the same material as the source and drain, including: using a co-sputtering method, using zinc oxide, tungsten, and aluminum as target materials, and forming the first zinc-aluminum-tungsten oxide layer in a preset area defined by a mask on the channel layer, wherein the sputtering power of the zinc oxide target is between 43.7-44.1 W, the sputtering power of the tungsten target is between 6.6-9.5 W, and the sputtering power of the aluminum target is between 10.2-1 8.9W; using radio frequency magnetron sputtering method, with silver as target, a silver layer is formed on the first zinc aluminum tungsten oxide layer, wherein the sputtering power of the silver target is between 80.5-80.9W; using co-sputtering method, with zinc oxide, tungsten and aluminum as target materials, a second zinc aluminum tungsten oxide layer is formed on the silver layer, wherein the sputtering power of the zinc oxide target is between 43.7-44.1W, the sputtering power of the tungsten target is between 6.6-9.5W, and the sputtering power of the aluminum target is between 10.2-18.9W.
[0007] As an practicable manner, the sputtering time of the first zinc aluminum tungsten oxide layer is between 12-13 minutes; the sputtering time of the silver layer is between 6-8 minutes; and the sputtering time of the second zinc aluminum tungsten oxide layer is between 13-15 minutes.
[0008] As an practicable method, a dielectric layer is formed on a channel layer having a source and a drain, wherein the dielectric layer is located between the source and the drain, including: dissolving organic polymethyl methacrylate in acetone to form a solution; spin coating the solution on the channel layer by spin coating and drying, wherein the spin coating speed is 6000 r / min, and baking at a temperature of 70-90°C for 30 minutes to form the dielectric layer.
[0009] As an practicable manner, the solution is spin-coated on the channel layer for multiple times and then dried.
[0010] As an practicable method, a flexible substrate is provided, and a channel layer is formed on the flexible substrate, including: providing a flexible substrate; using a co-sputtering method to form a zinc-tin-tungsten-lanthanum oxide layer as a channel layer on the flexible substrate using zinc-tin oxide, tungsten and lanthanum as targets, wherein the sputtering power of the zinc-tin oxide target is between 50-50.4W, the sputtering power of the tungsten target is between 5.1-5.5W, and the sputtering power of the lanthanum target is between 3.7-4.1.
[0011] On the other hand, an embodiment of the present application provides a thin film transistor, including a flexible substrate and a channel layer sequentially arranged on the flexible substrate, a source and a drain are spaced apart and arranged on the same layer and with the same material on the channel layer, a dielectric layer is formed on the channel layer on which the source and the drain are formed, the dielectric layer is located between the source and the drain, and a gate is formed on the dielectric layer, and the source and the drain both include a first zinc aluminum tungsten oxide layer, a silver layer, and a second zinc aluminum tungsten oxide layer sequentially arranged.
[0012] As an practicable manner, the thickness of the first zinc aluminum tungsten oxide layer is less than the thickness of the second zinc aluminum tungsten oxide layer.
[0013] As an practicable manner, the thickness of the first zinc aluminum tungsten oxide layer is between 44-48 nm, and the thickness of the second zinc aluminum tungsten oxide layer is between 52-56 nm.
[0014] As an practicable manner, in the first zinc-aluminum-tungsten oxide layer, the atomic percentage of aluminum is between 31.6 at.% and 40.7 at.%, and the atomic percentage of tungsten is between 16.1 at.% and 22.0 at.%; in the second zinc-aluminum-tungsten oxide layer, the atomic percentage of aluminum is between 31.6 at.% and 40.7 at.%, and the atomic percentage of tungsten is between 16.1 at.% and 22.0 at.%.
[0015] As an practicable manner, the material of the channel layer is zinc tin tungsten lanthanum oxide.
[0016] As an practicable manner, in the zinc-tin-tungsten-lanthanum oxide, the molar ratio of zinc to tin is 1:3, the atomic percentage of tungsten is 6.0 at.%, and the atomic percentage of lanthanum is 4.0 at.%.
[0017] As an practicable manner, the material of the dielectric layer is organic polymethyl methacrylate.
[0018] The beneficial effects of the embodiments of the present application include:
[0019] The method for preparing a thin film transistor provided in the present application comprises providing a flexible substrate and forming a channel layer on the flexible substrate; forming a first zinc-aluminum-tungsten oxide layer, a silver layer and a second zinc-aluminum-tungsten oxide layer of the same material in the same layer on the channel layer as a source electrode and a drain electrode; adding aluminum oxide to zinc oxide in the first zinc-aluminum-tungsten oxide layer and the second zinc-aluminum-tungsten oxide layer, and the aluminum oxide can inhibit the crystallization of zinc oxide, so that the first zinc-aluminum-tungsten oxide layer has a stable amorphous structure, so that a good physical contact is formed between the source electrode and the drain electrode and the channel layer, and at the same time, through the setting of the three-layer structure of the first zinc-aluminum-tungsten oxide layer, the silver layer and the second zinc-aluminum-tungsten oxide layer, a good energy level matching is formed between the source electrode and the drain electrode and the channel layer, so that the contact between the source electrode and the drain electrode and the channel layer is an ohmic contact, thereby improving the electrical performance; in addition, adding tungsten element to zinc oxide, the tungsten element and the zinc element have different electronegativity, so the tungsten element can inhibit the generation of oxygen vacancies in zinc oxide, thereby reducing the problem of oxygen adsorption caused by the source or drain electrode having more oxygen vacancies, thereby improving the stability of the source and the drain electrode. In addition, by setting up the three-layer structure of the first zinc aluminum tungsten oxide layer, the silver layer and the second zinc aluminum tungsten oxide layer, the source and drain electrodes themselves have a lower resistance, thereby improving the electrical performance of the source and drain electrodes. A dielectric layer is formed on the channel layer formed with the source and drain electrodes, and the dielectric layer is located between the source and drain electrodes; and a gate electrode is formed on the dielectric layer. Therefore, the embodiment of the present application can improve the bending stress stability and electrical performance of the source and drain electrodes. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 A flow chart of a method for preparing a thin film transistor provided in an embodiment of the present application;
[0022] Figure 2 One of the state diagrams of a thin film transistor provided in an embodiment of the present application;
[0023] Figure 3 The second state diagram of a thin film transistor provided in an embodiment of the present application;
[0024] Figure 4 The third state diagram of a thin film transistor provided in an embodiment of the present application;
[0025] Figure 5 A schematic diagram of the structure of a thin film transistor provided in an embodiment of the present application.
[0026] Icon: 110 - flexible substrate; 120 - channel layer; 130 - source; 140 - drain; 151 - first zinc aluminum tungsten oxide layer; 152 - silver layer; 153 - second zinc aluminum tungsten oxide layer; 160 - dielectric layer; 170 - gate. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. The components of the embodiments of the present application described and shown in the drawings here can be arranged and designed in various different configurations.
[0028] Therefore, the following detailed description of the embodiments of the present application provided in the accompanying drawings is not intended to limit the scope of the present application for which protection is sought, but merely represents selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.
[0029] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0030] The present application provides a method for preparing a thin film transistor, such as Figure 1 As shown, including:
[0031] S10: Figure 2 As shown, a flexible substrate 110 is provided, and a channel layer 120 is formed on the flexible substrate 110;
[0032] Specifically, the material of the flexible substrate 110 is not limited in the present embodiment of the application, and those skilled in the art can select it according to the actual situation, as long as it can meet the requirements of high light transmittance and high flexibility. The channel layer 120 has good semiconductor properties while meeting the requirements of high light transmittance and high flexibility. For example, the flexible substrate 110 can be polyethylene terephthalate.
[0033] S20: Figure 3 As shown, a first zinc aluminum tungsten oxide layer 151, a silver layer 152 and a second zinc aluminum tungsten oxide layer 153 of the same layer and the same material are sequentially formed on the channel layer 120 to serve as the source 130 and the drain 140;
[0034] Specifically, the source electrode 130 and the drain electrode 140 are spaced apart on the channel layer 120 , and both the source electrode 130 and the drain electrode 140 include a first zinc aluminum tungsten oxide layer 151 , a silver layer 152 , and a second zinc aluminum tungsten oxide layer 153 .
[0035] In the first zinc-aluminum-tungsten oxide layer 151 and the second zinc-aluminum-tungsten oxide layer 153 of the embodiment of the present application, aluminum oxide is added to zinc oxide. Aluminum oxide can inhibit the crystallization of zinc oxide, so that the first zinc-aluminum-tungsten oxide layer has a stable amorphous structure, so that the source electrode 130 and the drain electrode 140 form a good physical contact with the channel layer 120. At the same time, through the setting of the three-layer structure of the first zinc-aluminum-tungsten oxide layer 151, the silver layer 152 and the second zinc-aluminum-tungsten oxide layer 153, a good energy level matching is formed between the source electrode 130 and the drain electrode 140 and the channel layer 120, so that the contact between the source electrode 130 and the drain electrode 140 and the channel layer 120 is an ohmic contact, thereby improving the electrical performance; in addition, tungsten is added to zinc oxide. Tungsten and zinc have different electronegativity. Therefore, tungsten can inhibit the generation of oxygen vacancies in zinc oxide, thereby reducing the problem of oxygen adsorption caused by the source electrode 130 or the drain electrode 140 having more oxygen vacancies, thereby improving the stability of the source electrode 130 and the drain electrode 140. In addition, by setting up a three-layer structure of the first zinc aluminum tungsten oxide layer 151 , the silver layer 152 and the second zinc aluminum tungsten oxide layer 153 , the source 130 and the drain 140 themselves have lower resistance, thereby improving the electrical properties of the source 130 and the drain 140 .
[0036] Therefore, by configuring the source 130 and the drain 140 to be a three-layer structure, the materials and the hierarchical relationship of the three-layer structure enable the source 130 and the drain 140 of the embodiment of the present application to have higher bending stress stability and electrical performance.
[0037] In addition, the materials such as zinc, aluminum and tungsten contained in the first zinc aluminum tungsten oxide layer 151 and the second zinc aluminum tungsten oxide layer 153 do not contain precious metals such as indium and gallium. Therefore, the source 130 and the drain 140 of the embodiment of the present application can also reduce the cost of the thin film transistor.
[0038] S30: Figure 4 As shown, a dielectric layer 160 is formed on the channel layer 120 on which the source 130 and the drain 140 are formed, and the dielectric layer 160 is located between the source 130 and the drain 140;
[0039] S40: Figure 5 As shown, a gate 170 is formed on the dielectric layer 160 .
[0040] The gate 170 is used as a switch to control the flow channel between the source 130 and the drain 140. Specifically, the gate 170 can be prepared by radio frequency magnetron sputtering. More specifically, a zinc aluminum oxide layer is formed in the preset area defined by a mask on the dielectric layer 160 using zinc aluminum oxide ceramic as a target material as the gate 170, with a thickness of 80-150 nm. During the sputtering process, the sputtering power is 40-55 W, and the argon working pressure is 0.5-1.2 Pa. The purity of the target zinc aluminum oxide ceramic can be 4N, and the aluminum atomic percentage is 3.0 at.%.
[0041] In the embodiment of the present application, a first zinc-aluminum-tungsten oxide layer 151, a silver layer 152, and a second zinc-aluminum-tungsten oxide layer 153 are sequentially formed of the same layer and the same material in two regions on the channel layer 120 as the source 130 and the drain 140. By setting the three-layer structure of the first zinc-aluminum-tungsten oxide layer 151, the silver layer 152, and the second zinc-aluminum-tungsten oxide layer 153, the source 130 and the drain 140 themselves have a lower resistance. In addition, in the first zinc-aluminum-tungsten oxide layer 151 and the second zinc-aluminum-tungsten oxide layer 153, the bending stress stability and electrical performance of the source 130 and the drain 140 of the thin film transistor can be improved through the regulating effect of aluminum and tungsten.
[0042] Optionally, a first zinc aluminum tungsten oxide layer 151, a silver layer 152, and a second zinc aluminum tungsten oxide layer 153 are sequentially formed on the channel layer 120 in the same layer and with the same material as the source 130 and the drain 140, including:
[0043] S21: using a co-sputtering method, zinc oxide, tungsten and aluminum as target materials, respectively forming a first zinc-aluminum-tungsten oxide layer 151 in a preset area defined by a mask on the channel layer 120, wherein the sputtering power of the zinc oxide target is between 43.7-44.1 W, the sputtering power of the tungsten target is between 6.6-9.5 W, and the sputtering power of the aluminum target is between 10.2-18.9 W;
[0044] Specifically, the first zinc-aluminum-tungsten oxide layer 151 is prepared at room temperature by co-sputtering of radio frequency magnetron sputtering and direct current magnetron sputtering, the target materials are zinc oxide, tungsten and aluminum, and argon gas is introduced as a collision gas. The pressure of the argon gas is 0.7 Pa. Since the source 130 and the drain 140 are to be formed on the channel layer 120, the mask defines two regions on the channel layer 120, so that the first zinc-aluminum-tungsten oxide layer 151 is formed in the two regions.
[0045] For example, the sputtering power of the zinc oxide target is 43.9W, the sputtering power of the tungsten target is 8.3W, and the sputtering power of the aluminum target is 12.6W.
[0046] S22: using a radio frequency magnetron sputtering method and taking silver as a target material, forming a silver layer 152 on the first zinc aluminum tungsten oxide layer 151, wherein the sputtering power of the silver target material is between 80.5 W and 80.9 W;
[0047] Similarly, a silver layer 152 is formed on the first zinc aluminum tungsten oxide layer 151 using a mask. The sputtering power may be 80.7 W, and the working pressure of the argon gas may be 0.7 Pa.
[0048] S23: A co-sputtering method is adopted with zinc oxide, tungsten and aluminum as targets to form a second zinc-aluminum-tungsten oxide layer 153 on the silver layer 152, wherein the sputtering power of the zinc oxide target is between 43.7-44.1 W, the sputtering power of the tungsten target is between 6.6-9.5 W, and the sputtering power of the aluminum target is between 10.2-18.9 W.
[0049] Similar to the first zinc aluminum tungsten oxide layer 151 , the second zinc aluminum tungsten oxide layer 153 is prepared at room temperature by co-sputtering of RF magnetron sputtering and DC magnetron sputtering. During the co-sputtering process, the parameters are the same as those of the first zinc aluminum tungsten oxide layer 151 .
[0050] In one achievable manner of the embodiment of the present application, the sputtering time of the first zinc aluminum tungsten oxide layer 151 is between 12-13 minutes; the sputtering time of the silver layer 152 is between 6-8 minutes; and the sputtering time of the second zinc aluminum tungsten oxide layer 153 is between 13-15 minutes.
[0051] By controlling the sputtering time of each layer, the thickness of the first zinc aluminum tungsten oxide layer is between 44-48nm, the thickness of the silver layer 152 is between 10-12mm, and the thickness of the second zinc aluminum tungsten oxide layer 153 is between 52-56nm. The setting of the thickness of each layer reduces the reflection of visible light by the source 130 and the drain 140, and also effectively inhibits the surface plasma coupling at the cross section of the first zinc aluminum tungsten oxide layer and the second zinc aluminum tungsten oxide layer and the silver layer 152, thereby reducing the absorption of visible light by the source 130 and the drain 140. Based on the source 130 and the drain 140, the reflection of visible light by the source 130 and the drain 140 and the absorption of visible light by the source 130 and the drain 140 can be reduced, so that the source 130 and the drain 140 have a higher visible light transmittance.
[0052] Optionally, a dielectric layer 160 is formed on the channel layer 120 on which the source 130 and the drain 140 are formed, and the dielectric layer 160 is located between the source 130 and the drain 140, and includes:
[0053] S31: dissolving organic polymethyl methacrylate in acetone to form a solution;
[0054] The concentration of the solution is 30 mg / mL of organic polymethyl methacrylate solution.
[0055] S32: Spin-coat the solution onto the channel layer 120 and dry it, wherein the spin-coating speed is 6000 r / min, and bake it at a temperature of 70-90° C. for 30 minutes to form the dielectric layer 160 .
[0056] Organic matter is used as the dielectric layer 160, and a solution spin coating method can be used for preparation, so that the temperature during preparation is lower than 100°C. This is compatible with the preparation process of top-gate coplanar structure devices, and the thin film transistor can be set as a top-gate coplanar structure device. This avoids the bottom gate structure in the prior art being exposed to the air, which is easy to react with water and oxygen and makes the performance of the thin film transistor unstable.
[0057] Specifically, the thickness of the dielectric layer 160 may be 160 nm.
[0058] In one achievable manner of the embodiment of the present application, the solution is spin-coated on the channel layer 120 multiple times and then dried.
[0059] The spin coating solution and the drying cycle are repeated multiple times to form a dielectric layer 160 with a preset thickness, so that the thickness of the film formed each time is smaller. In this way, cracks are less likely to occur during the drying process, so that the dielectric layer 160 has a better surface morphology.
[0060] Optionally, providing a flexible substrate 110 and forming a channel layer 120 on the flexible substrate 110 includes:
[0061] S11: providing a flexible substrate 110;
[0062] S12: A co-sputtering method is adopted to form a zinc-tin-tungsten-lanthanum oxide layer as a channel layer 120 on the flexible substrate 110 using zinc-tin oxide, tungsten and lanthanum as targets, wherein the sputtering power of the zinc-tin oxide target is between 50-50.4 W, the sputtering power of the tungsten target is between 5.1-5.5 W, and the sputtering power of the lanthanum target is between 3.7-4.1.
[0063] Specifically, the co-sputtering method of RF magnetron sputtering and DC magnetron sputtering was used. During the co-sputtering process, the sputtering power of the zinc oxide tin target was 50.2W, the sputtering power of the tungsten target was 5.3W, the sputtering power of the lanthanum target was 3.9W, and the oxygen partial pressure was (2*10 -2 pa) remains unchanged, the argon pressure is 0.5-1.0 pa, and the total sputtering time is 25-36 min.
[0064] The thickness of the channel layer 120 is 80 nm.
[0065] A zinc-tin-tungsten-lanthanum oxide layer is used as the channel layer 120. Based on the adjustment of the zinc-tin oxide by tungsten and lanthanum components, the zinc-tin-tungsten-lanthanum oxide layer can accurately regulate the carrier concentration in the channel layer 120, thereby improving the mobility of the thin film transistor and reducing the threshold voltage and off-state current.
[0066] In order to further verify the beneficial effects of the embodiments of the present application, the visible light transmittance, mobility, threshold voltage, off-state current and bending stress stability of the thin film transistor of the embodiments of the present application were measured. The measurement results are as follows: the visible light transmittance is higher than 90%, the mobility is higher than 70cm 2 / Vs, the threshold voltage is close to 0V and the off-state current is less than 10 -10 A; when the radius of curvature is greater than or equal to 10 mm, after the thin film transistor is bent 500 times, its threshold voltage changes by ±0.2 V. Therefore, the thin film transistor prepared by the thin film transistor preparation method provided in the embodiment of the present application has good electrical properties, light transmittance, and good bending stress stability.
[0067] The embodiment of the present application also discloses a thin film transistor, including a flexible substrate 110 and a channel layer 120 sequentially arranged on the flexible substrate 110, wherein a source 130 and a drain 140 are spaced apart and arranged on the same layer and with the same material on the channel layer 120, a dielectric layer 160 is formed on the channel layer 120 on which the source 130 and the drain 140 are formed, the dielectric layer 160 is located between the source 130 and the drain 140, and a gate 170 is formed on the dielectric layer 160, and the source 130 and the drain 140 both include a first zinc aluminum tungsten oxide layer 151, a silver layer 152 and a second zinc aluminum tungsten oxide layer 153 sequentially arranged.
[0068] The source electrode 130 and the drain electrode 140 are set to a three-layer structure, wherein the first zinc aluminum tungsten oxide layer 151 and the second zinc aluminum tungsten oxide layer 153 are provided. Aluminum oxide is added to zinc oxide. Aluminum oxide can inhibit the crystallization of zinc oxide, so that the first zinc aluminum tungsten oxide layer has a stable amorphous structure, thereby forming a good physical contact between the source electrode 130 and the drain electrode 140 and the channel layer 120. At the same time, the three-layer structure of the first zinc aluminum tungsten oxide layer 151, the silver layer 152 and the second zinc aluminum tungsten oxide layer 153 is provided. A good energy level match is formed between the source 130 and the drain 140 and the channel layer 120, so that the contact between the source 130 and the drain 140 and the channel layer 120 is an ohmic contact, thereby improving the electrical performance; in addition, tungsten is added to zinc oxide, and tungsten and zinc have different electronegativity, so tungsten can inhibit the generation of oxygen vacancies in zinc oxide, thereby reducing the problem of oxygen adsorption caused by more oxygen vacancies in the source 130 or the drain 140, thereby improving the stability of the source 130 and the drain 140. In addition, by setting the three-layer structure of the first zinc aluminum tungsten oxide layer 151, the silver layer 152 and the second zinc aluminum tungsten oxide layer 153, the source 130 and the drain 140 themselves have a lower resistance, thereby improving the electrical performance of the source 130 and the drain 140.
[0069] In one achievable manner of the embodiment of the present application, the thickness of the first zinc aluminum tungsten oxide layer 151 is less than the thickness of the second zinc aluminum tungsten oxide layer 153 .
[0070] The thickness of the first zinc aluminum tungsten oxide layer 151 is smaller than that of the second zinc aluminum tungsten oxide layer 153 , and when visible light passes through the source electrode 130 or the drain electrode 140 , the transmittance of the source electrode 130 and the drain electrode 140 to visible light can be increased.
[0071] Optionally, the thickness of the first zinc aluminum tungsten oxide layer 151 is between 44-48 nm, and the thickness of the second zinc aluminum tungsten oxide layer 153 is between 52-56 nm.
[0072] Based on the functions of the source 130 and the drain 140 and the three-layer structure design, when the thickness of the first zinc aluminum tungsten oxide layer 151 is between 44-48nm and the thickness of the second zinc aluminum tungsten oxide layer 153 is between 52-56nm, the source 130 and the drain 140 have a higher transmittance to visible light.
[0073] Preferably, when the thickness of the first zinc aluminum tungsten oxide layer is 46 nm and the thickness of the second zinc aluminum tungsten oxide layer 153 is 54 nm, the transmittance of the source electrode 130 and the drain electrode 140 to visible light is the highest.
[0074] In one achievable method of an embodiment of the present application, in the first zinc aluminum tungsten oxide layer 151, the atomic percentage of aluminum is between 31.6 at.% and 40.7 at.%, and the atomic percentage of tungsten is between 16.1 at.% and 22.0 at.%; in the second zinc aluminum tungsten oxide layer 153, the atomic percentage of aluminum is between 31.6 at.% and 40.7 at.%, and the atomic percentage of tungsten is between 16.1 at.% and 22.0 at.%.
[0075] Based on the first zinc aluminum tungsten oxide layer 151 and the second zinc aluminum tungsten oxide layer 153, aluminum oxide can inhibit the crystallization of zinc oxide, so that the first zinc aluminum tungsten oxide layer has a stable amorphous structure; tungsten and zinc have different electronegativity, so tungsten can inhibit the generation of oxygen vacancies in zinc oxide, thereby reducing the problem of oxygen adsorption caused by more oxygen vacancies in the source 130 or the drain 140. When the atomic percentage of aluminum is between 31.6at.% and 40.7at.%, and the atomic percentage of tungsten is between 16.1at.% and 22.0at.%, the improvement effect on the source 130 and the drain 140 is better.
[0076] Optionally, the material of the channel layer 120 is zinc tin tungsten lanthanum oxide.
[0077] A zinc-tin-tungsten-lanthanum oxide layer is used as the channel layer 120. Based on the adjustment of the zinc-tin oxide by tungsten and lanthanum components, the zinc-tin-tungsten-lanthanum oxide layer can accurately regulate the carrier concentration in the channel layer 120, thereby improving the mobility of the thin film transistor and reducing the threshold voltage and off-state current.
[0078] In one achievable manner of the embodiment of the present application, in the zinc-tin-tungsten-lanthanum oxide, the molar ratio of zinc to tin is 1:3, the atomic percentage of tungsten is 6.0 at.%, and the atomic percentage of lanthanum is 4.0 at.%.
[0079] Based on the adjustment of tungsten and lanthanum components to zinc tin oxide, when the tungsten atomic percentage is 6.0 at. % and the lanthanum atomic percentage is 4.0 at. %, the channel layer 120 has better electrical properties.
[0080] Optionally, the material of the dielectric layer 160 is organic polymethyl methacrylate.
[0081] The material of the dielectric layer 160 is organic polymethyl methacrylate, which can be prepared by a solution spin coating method so that the temperature during preparation is lower than 100°C. This makes it compatible with the preparation process of top-gate coplanar structure devices, and the thin-film transistor can be set as a top-gate coplanar structure device. This avoids the bottom gate structure in the prior art being exposed to the air, which is easy to react with water and oxygen and makes the performance of the thin-film transistor unstable.
[0082] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A method for preparing a thin film transistor, characterized in that: include: Providing a flexible substrate, and forming a channel layer on the flexible substrate; On the channel layer, a first zinc aluminum tungsten oxide layer, a silver layer, and a second zinc aluminum tungsten oxide layer are sequentially formed in the same layer and material as a source electrode and a drain electrode; forming a dielectric layer on the channel layer on which the source electrode and the drain electrode are formed, wherein the dielectric layer is located between the source electrode and the drain electrode; A gate is formed on the dielectric layer.
2. The method for preparing a thin film transistor according to claim 1, characterized in that: The first zinc aluminum tungsten oxide layer, the silver layer and the second zinc aluminum tungsten oxide layer in the same layer and material on the channel layer are used as the source and drain, including: A co-sputtering method is adopted, with zinc oxide, tungsten and aluminum as target materials, and a first zinc-aluminum-tungsten oxide layer is formed in preset areas defined by a mask on the channel layer, wherein the sputtering power of the zinc oxide target is between 43.7-44.1 W, the sputtering power of the tungsten target is between 6.6-9.5 W, and the sputtering power of the aluminum target is between 10.2-18.9 W; A radio frequency magnetron sputtering method is adopted, with silver as a target material, to form a silver layer on the first zinc-aluminum-tungsten oxide layer, wherein the sputtering power of the silver target material is between 80.5 W and 80.9 W; A co-sputtering method is adopted with zinc oxide, tungsten and aluminum as targets to form a second zinc-aluminum-tungsten oxide layer on the silver layer, wherein the sputtering power of the zinc oxide target is between 43.7-44.1 W, the sputtering power of the tungsten target is between 6.6-9.5 W, and the sputtering power of the aluminum target is between 10.2-18.9 W.
3. The method for preparing a thin film transistor according to claim 1, characterized in that: The sputtering time of the first zinc-aluminum-tungsten oxide layer is between 12-13 minutes; the sputtering time of the silver layer is between 6-8 minutes; and the sputtering time of the second zinc-aluminum-tungsten oxide layer is between 13-15 minutes.
4. The method for preparing a thin film transistor according to claim 1, characterized in that: The step of forming a dielectric layer on the channel layer having the source and the drain, wherein the dielectric layer is located between the source and the drain, comprises: dissolving organic polymethyl methacrylate in acetone to form a solution; The solution is spin-coated on the channel layer by a spin coating method and dried, wherein the spin coating speed is 6000 r / min, and the solution is baked at a temperature of 70-90° C. for 30 minutes to form a dielectric layer.
5. The method for preparing a thin film transistor according to claim 1, characterized in that: The step of providing a flexible substrate and forming a channel layer on the flexible substrate comprises: providing a flexible substrate; A co-sputtering method is adopted to form a zinc-tin-tungsten-lanthanum oxide layer as a channel layer on the flexible substrate using zinc-tin oxide, tungsten and lanthanum as targets, wherein the sputtering power of the zinc-tin oxide target is between 50-50.4W, the sputtering power of the tungsten target is between 5.1-5.5W, and the sputtering power of the lanthanum target is between 3.7-4.
1.
6. A thin film transistor, characterized in that: The invention comprises a flexible substrate and a channel layer sequentially arranged on the flexible substrate, wherein a source electrode and a drain electrode are spaced apart and arranged on the channel layer in the same layer and with the same material, a dielectric layer is formed on the channel layer on which the source electrode and the drain electrode are formed, the dielectric layer is located between the source electrode and the drain electrode, and a gate electrode is also formed on the dielectric layer, and the source electrode and the drain electrode both comprise a first zinc-aluminum-tungsten oxide layer, a silver layer and a second zinc-aluminum-tungsten oxide layer sequentially arranged.
7. The thin film transistor according to claim 6, characterized in that: The thickness of the first zinc aluminum tungsten oxide layer is smaller than the thickness of the second zinc aluminum tungsten oxide layer.
8. The thin film transistor according to claim 7, characterized in that: The thickness of the first zinc-aluminum-tungsten oxide layer is between 44-48 nm, and the thickness of the second zinc-aluminum-tungsten oxide layer is between 52-56 nm; In the second zinc-aluminum-tungsten oxide layer, the atomic percentage of aluminum is between 31.6 at.% and 40.7 at.%, and the atomic percentage of tungsten is between 16.1 at.% and 22.0 at.%.
9. The thin film transistor according to claim 6, characterized in that: The material of the channel layer is zinc, tin, tungsten and lanthanum oxide.
10. The thin film transistor according to claim 6, characterized in that: The material of the dielectric layer is organic polymethyl methacrylate.