Lithium phosphate coated and modified silicon-carbon negative electrode material and preparation method thereof

By coating the modified silicon carbon negative electrode material with lithium phosphate, and using CVD vapor deposition and liquid phase coating technology, a porous core-shell structure is formed, solving the performance problems of silicon carbon material due to volume expansion rate and specific surface area in lithium-ion batteries. , achieving high specific capacity, good cycle stability and low cost effects.

CN118983425AInactive Publication Date: 2024-11-19SHAANXI JINGTAI NEW ENERGY TECH CO LTD

Patent Information

Application Number
CN202411422779.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Silicon-carbon negative electrode material is caused by structural damage and electrochemical performance in lithium-ion batteries due to high volume expansion and large specific surface area. It is difficult for traditional coating technology to achieve uniform and cost-effective surface treatment, which limits the improvement of material performance.

Method used

Using lithium phosphate-coated modified silicon carbon anode material, through CVD vapor deposition and liquid phase coating technology, silicon carbon material with porous core-shell structure is formed, reducing specific surface area, improving cycle stability and electrochemical performance, and simplifying production Process to reduce costs.

Benefits of technology

It significantly reduces the specific surface area of ​​silicon-carbon anode material, improves the magnification and cycle stability, reduces production costs, and has good environmental friendliness, is suitable for industrial production, has a wide application prospect and market competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983425A_ABST
    Figure CN118983425A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium phosphate coated and modified silicon-carbon negative electrode material and a preparation method thereof, and belongs to the technical field of negative electrode materials and preparation of the negative electrode materials. And then carrying out surface coating modification on the silicon-carbon negative electrode material through a lithium phosphate liquid-phase coating process. According to the lithium phosphate coated and modified silicon-carbon negative electrode material and the preparation method thereof, the problem of performance limitation of the silicon-carbon negative electrode material in the application of a lithium ion battery is effectively solved, and the prepared high-specific-capacity lithium ion battery negative electrode material has the advantages that the specific surface area of the silicon-carbon negative electrode material is obviously reduced; compared with the prior art, the preparation method provided by the invention has the advantages that the rate and cycling stability are improved, the production cost is reduced, good environmental friendliness is achieved, and wide application prospects and market competitiveness are achieved in the field of lithium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of negative electrode materials and preparation thereof, and in particular to a lithium phosphate coated modified silicon-carbon negative electrode material and a preparation method thereof. Background Art

[0002] In the prior art, although silicon-carbon negative electrode materials have high capacity, the high volume expansion rate of silicon causes the material to be easily damaged during the charge and discharge cycle, affecting the cycle stability of the battery. In addition, the large specific surface area of ​​silicon-carbon materials increases the side reactions with the electrolyte, resulting in a decrease in electrochemical performance. Traditional coating technology is difficult to achieve uniform and cost-effective surface treatment, further limiting the improvement of the performance of silicon-carbon materials. Summary of the invention

[0003] The purpose of the present invention is to provide a lithium phosphate coated modified silicon-carbon negative electrode material and a preparation method thereof, so as to effectively solve the performance limitation problem of silicon-carbon negative electrode material in lithium ion battery applications. The prepared high specific capacity lithium ion battery negative electrode material not only significantly reduces the specific surface area of ​​the silicon-carbon negative electrode material, improves its rate and cycle stability, but also reduces the production cost, and has good environmental friendliness, and has broad application prospects and market competitiveness in the field of lithium ion batteries.

[0004] To achieve the above-mentioned purpose, the present invention provides a lithium phosphate-coated modified silicon-carbon negative electrode material, wherein the silicon-carbon negative electrode material is a porous core-shell structure, comprising a silicon-carbon precursor material and a lithium phosphate coating layer coated on the outer layer of the silicon-carbon precursor material, wherein the silicon-carbon precursor material is composed of a porous carbon matrix and nano-silicon particles deposited in the pores and surface of the porous carbon matrix.

[0005] Preferably, the diameter of the silicon-carbon negative electrode material is 1-20 μm, wherein silicon accounts for 30-60% of the silicon-carbon negative electrode material, carbon accounts for 30-60% of the silicon-carbon negative electrode material, and lithium phosphate accounts for 1-10% of the silicon-carbon negative electrode material.

[0006] The present invention provides a method for preparing a lithium phosphate-coated modified silicon-carbon negative electrode material, comprising the following steps: S1. Preparing silicon-carbon precursor material by CVD vapor deposition equipment; S2, performing liquid phase coating optimization on the silicon-carbon precursor material prepared in S1 to obtain a modified silicon-carbon material; S3. Treat the modified silicon-carbon material solution obtained in S2 to obtain a lithium phosphate-coated modified silicon-carbon negative electrode material.

[0007] Preferably, the specific operation of S1 is: placing the porous carbon material into a CVD vapor deposition device, introducing silane gas into the device, and under high temperature conditions, the silane in the device is cracked into silicon atoms which are gradually deposited on the porous carbon material, and at the same time a small amount of carbon source gas is introduced to deposit a thin carbon layer, and then the temperature is reduced and the material is discharged to form a silicon-carbon precursor material.

[0008] Preferably, the specific operation of S2 is: dissolving the silicon-carbon precursor material obtained in S1 in a solvent and adding a phosphoric acid source, stirring the solution, adding a lithium hydroxide solution, allowing the phosphoric acid source and lithium hydroxide to react to generate lithium phosphate to coat the surface of the silicon-carbon precursor, thereby obtaining a modified silicon-carbon material.

[0009] Preferably, the specific operation of S3 is: filtering the solution of the modified silicon-carbon material obtained in S2 to obtain a modified silicon-carbon mixed powder material, then calcining it under a high-temperature protective atmosphere, and obtaining a finished silicon-carbon material after cooling.

[0010] Preferably, the specific operation of S3 is: filtering the solution of the modified silicon-carbon material obtained in S2 to obtain a modified silicon-carbon mixed powder material, and then drying it in a high-temperature drying oven at 80-120° C. for 1-3 hours, and obtaining a finished silicon-carbon material after cooling.

[0011] Preferably, the CVD vapor deposition equipment in S1 is one or both of a rotary furnace and a fluidized bed, the deposition temperature of the silane and the carbon source in S1 is 500-800°C, the deposition time is 0.5-24h, the porous carbon-based material is one or more of coconut shell carbon, resin carbon, and petroleum coke, and the carbon source gas is one or more of methane, ethane, acetylene, and propylene.

[0012] Preferably, the phosphate source in S2 is one or more of lithium dihydrogen phosphate, dilithium hydrogen phosphate, sodium dihydrogen phosphate and ammonium dihydrogen phosphate, and the solvent is one or both of water and ethanol.

[0013] Preferably, the protective atmosphere in S3 is one or more of nitrogen, argon, and argon-hydrogen mixed gas, the calcination temperature is 500-800° C., and the calcination time is 0.5-24 h.

[0014] Therefore, the present invention adopts the above-mentioned lithium phosphate coated modified silicon-carbon negative electrode material and its preparation method, which has the following beneficial effects: (1) Silicon material was deposited on porous carbon material by a simple and easy method, and then lithium phosphate liquid phase coating was carried out on this basis to prepare a silicon-carbon negative electrode material with a porous core-shell structure. This not only significantly reduced the specific surface area of ​​the silicon-carbon negative electrode material, but also improved its rate and cycle stability. The preparation process is simple and suitable for industrial production.

[0015] (2) The CVD vapor deposition process used in the present invention controls the gas source flow rate, deposition temperature, and deposition time to uniformly mix the porous carbon powder and the silane material in the gas phase and perform a pyrolysis reaction. This method can ensure the uniform distribution of silicon and carbon to form a silicon-carbon composite material with a stable structure. At the same time, it can provide uniform heat and gas distribution, so that the material is heated uniformly during the preparation process, thereby ensuring the uniform structure and performance of the silicon-carbon composite material.

[0016] (3) Liquid phase coating technology is used to modify the surface of the prepared silicon-carbon material. The advantages of liquid phase coating technology are that it is easy to operate, low cost, and can achieve large-area uniform coating. The silicon-carbon material is coated in a solution, and by controlling the amount of reaction raw materials and the reaction mode, lithium phosphate forms a uniform coating layer on the surface of the silicon-carbon material to achieve the effect of plugging pores, thereby reducing the specific surface area. At the same time, this coating layer can also reduce the direct contact between the silicon-carbon material and the electrolyte, reduce the occurrence of side reactions, and thus maintain good cycle stability and electrochemical performance.

[0017] (4) Controlling the generation of lithium phosphate by reaction and performing liquid phase coating. First, reaction control can better achieve the particle size control of lithium phosphate. Second, lithium phosphate, as a fast ion conductor, can improve the Li + The transmission rate is increased while optimizing the transmission path of lithium ions, thereby improving the charge and discharge efficiency and power density of the battery, allowing the material to further improve its rate performance.

[0018] (5) The CVD vapor deposition process can achieve continuous production, greatly improving production efficiency. At the same time, the liquid phase coating technology is easy to operate and does not require complex equipment and processes, further reducing production costs. These factors work together to make the technology of the present invention have significant cost advantages in industrial large-scale production. At the same time, the CVD process and liquid phase coating technology used in the present invention are both environmentally friendly production processes. The former generates less waste gas and waste residue during the preparation process and is easy to handle; the solvent used in the latter can be recycled and reused, reducing the discharge of chemical waste liquid.

[0019] (6) It has a significant gain effect and effectively solves the performance limitation problem of silicon-carbon negative electrode materials in lithium-ion battery applications. The prepared high specific capacity lithium-ion battery negative electrode materials not only significantly reduce the specific surface area of ​​silicon-carbon negative electrode materials, improve their rate and cycle stability, but also reduce production costs and have good environmental friendliness. It has broad application prospects and market competitiveness in the field of lithium-ion batteries.

[0020] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a flow chart of an embodiment of a lithium phosphate coated modified silicon-carbon negative electrode material and a preparation method thereof of the present invention; Figure 2 It is a schematic cross-sectional structure diagram of a lithium phosphate-coated modified silicon-carbon negative electrode material and a preparation method embodiment of the present invention. DETAILED DESCRIPTION

[0022] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0023] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0024] Example

[0025] like Figure 2 As shown, the present invention provides a lithium phosphate coated modified silicon-carbon negative electrode material, the silicon-carbon negative electrode material is a porous core-shell structure, including a silicon-carbon precursor material and a lithium phosphate coating layer coated on the outer layer of the silicon-carbon precursor material, wherein the silicon-carbon precursor material is composed of a porous carbon matrix and nano-silicon particles deposited in the pores and surface of the porous carbon matrix.

[0026] The diameter of the silicon-carbon negative electrode material is 1-20μm, of which silicon accounts for 30-60% of the silicon-carbon negative electrode material, carbon accounts for 30-60% of the silicon-carbon negative electrode material, and lithium phosphate accounts for 1-10% of the silicon-carbon negative electrode material.

[0027] like Figure 1 As shown, the present invention provides a method for preparing a lithium phosphate-coated modified silicon-carbon negative electrode material, comprising the following steps: S1. Prepare silicon-carbon precursor material by CVD vapor deposition equipment; put porous carbon material into CVD vapor deposition equipment, introduce silane gas into the equipment, under high temperature conditions, silane in the equipment is cracked into silicon atoms and gradually deposited on the porous carbon material, and a small amount of carbon source gas is introduced at the same time to deposit a thin carbon layer, and then the material is cooled and discharged to form silicon-carbon precursor material. Among them, the CVD vapor deposition equipment is one or two of a rotary kiln and a fluidized bed, the deposition temperature of silane and carbon source in S1 is 500-800℃, and the deposition time is 0.5-24h. The porous carbon-based material is one or more of coconut shell carbon, resin carbon, and petroleum coke, and the carbon source gas is one or more of methane, ethane, acetylene, and propylene.

[0028] The CVD vapor deposition process controls the gas source flow, deposition temperature, and deposition time to evenly mix the porous carbon powder and silane material in the gas phase and perform a pyrolysis reaction. This method can ensure the uniform distribution of silicon and carbon to form a structurally stable silicon-carbon composite material. At the same time, it can provide uniform heat and gas distribution, so that the material is evenly heated during the preparation process, thereby ensuring the uniform structure and performance of the silicon-carbon composite material.

[0029] S2, performing liquid phase coating optimization on the silicon-carbon precursor material obtained in S1 to obtain a modified silicon-carbon material; dissolving the silicon-carbon precursor material obtained in S1 in a solvent and adding a phosphoric acid source, stirring the solution, adding a lithium hydroxide solution, and reacting the phosphoric acid source and lithium hydroxide to generate lithium phosphate to coat the surface of the silicon-carbon precursor, thereby obtaining a modified silicon-carbon material. The phosphoric acid source is one or more of lithium dihydrogen phosphate, dilithium hydrogen phosphate, sodium dihydrogen phosphate and ammonium dihydrogen phosphate, and the solvent is one or both of water and ethanol.

[0030] The prepared silicon-carbon material is surface modified by liquid-phase coating technology. The advantages of liquid-phase coating technology are that it is easy to operate, low-cost, and can achieve uniform coating over a large area. The silicon-carbon material is coated in a solution, and by controlling the amount of reaction raw materials and the reaction mode, lithium phosphate forms a uniform coating layer on the surface of the silicon-carbon material to achieve the effect of plugging pores, thereby reducing the specific surface area. At the same time, this coating layer can also reduce the direct contact between the silicon-carbon material and the electrolyte, reduce the occurrence of side reactions, and thus maintain good cycle stability and electrochemical performance.

[0031] By controlling the generation of lithium phosphate through reaction and performing liquid phase coating, firstly, reaction control can better achieve the particle size control of lithium phosphate. Secondly, lithium phosphate, as a fast ion conductor, can improve the Li + The transmission rate is increased while optimizing the transmission path of lithium ions, thereby improving the charge and discharge efficiency and power density of the battery, allowing the material to further improve its rate performance.

[0032] S3, treating the modified silicon-carbon material solution obtained in S2 to obtain a lithium phosphate-coated modified silicon-carbon negative electrode material, the treatment method being: filtering the modified silicon-carbon material solution obtained in S2 to obtain a modified silicon-carbon mixed powder material, and then calcining it under a high-temperature protective atmosphere, and cooling it to obtain a finished silicon-carbon material. The protective atmosphere is one or more of nitrogen, argon, and argon-hydrogen mixed gas, the calcination temperature is 500-800°C, and the calcination time is 0.5-24h.

[0033] Example 1

[0034] (1) 1 kg of coconut shell porous carbon material was placed in a fluidized bed device, and 3 L / min of silane gas was introduced into the device. At a high temperature of 600 °C, silane was cracked to form elemental silicon, which was attached to the porous carbon pores and surface. The silane deposition time was 5 h. Then 3 L / min of acetylene gas was introduced into the device for carbon coating. The deposition time was 1 h. After cooling, the silicon-carbon precursor material was obtained.

[0035] (2) Take 1 kg of the silicon-carbon precursor material in step (1) to prepare a 20% by mass ratio silicon-carbon precursor material aqueous solution, then add 50 g of lithium dihydrogen phosphate and stir for 30 minutes to mix the solution evenly. Then, 30 g of lithium hydroxide is first prepared into a 20% lithium hydroxide aqueous solution, and then the lithium hydroxide solution is slowly added to the silicon-carbon precursor material solution to react the lithium dihydrogen phosphate and lithium hydroxide to generate lithium phosphate, and the solution is stirred for 30 minutes to mix the components evenly.

[0036] (3) The solution in step (2) is filtered, and then the powder obtained by filtration is dried in a high-temperature drying oven at 100° C. for 2 h, thereby finally obtaining a lithium phosphate-coated silicon-carbon negative electrode material.

[0037] Performance test of silicon-carbon negative electrode material: Specific surface area test: 2g of silicon-carbon negative electrode material was baked for 2h and tested using a BEST 2000A specific surface area tester. The test results are shown in Table 1.

[0038] Button test: Grind the silicon-carbon negative electrode material, conductive agent SP and adhesive CMC into slurry in a mass ratio of 8:1:1, and then apply the mixed electrode material on copper foil to make a pole piece. Dry the pole piece in a vacuum drying oven at 80°C for 12 hours, and then punch it into a Ø16mm circular pole piece. Use the punched Ø16mm pole piece as the positive electrode and the metal lithium sheet as the negative electrode to assemble a CR2032 button half-cell. The charge and discharge cut-off voltages are 1.5V and 0.005V, respectively. After the battery is activated by charging and discharging for 3 times at a current density of 0.1C, its rate performance is tested at a current density of 1C, and then the cycle stability test is carried out at a current density of 0.5C. The specific capacity, first efficiency, rate and cycle retention rate obtained from the test are shown in Table 1.

[0039] Example 2

[0040] (1) 1 kg of petroleum coke porous carbon material was placed in a fluidized bed device, and 3 L / min of silane gas was introduced into the device. At a high temperature of 600 °C, silane was cracked to form elemental silicon, which was attached to the porous carbon pores and surface. The silane deposition time was 5 hours. Then 3 L / min of acetylene gas was introduced into the device for carbon coating. The deposition time was 1 hour. After cooling, the silicon-carbon precursor material was obtained.

[0041] (2) Take 1 kg of the silicon-carbon precursor material in step (1) to prepare a 20% by mass ratio silicon-carbon precursor material aqueous solution, then add 50 g of sodium dihydrogen phosphate and stir for 30 minutes to mix the solution evenly. Then, 30 g of lithium hydroxide is first prepared into a 20% lithium hydroxide aqueous solution, and then the lithium hydroxide solution is slowly added to the aforementioned silicon-carbon negative electrode solution to react sodium dihydrogen phosphate and lithium hydroxide to generate lithium phosphate, and the solution is stirred for 30 minutes to mix the components evenly.

[0042] (3) The solution in step (2) is filtered, and then the powder obtained by filtration is dried in a high-temperature drying oven at 100° C. for 2 h, thereby finally obtaining a lithium phosphate-coated silicon-carbon negative electrode material.

[0043] The performance test method of the silicon-carbon negative electrode material is the same as that in Example 1, and the test results are shown in Table 1.

[0044] Example 3

[0045] (1) 1 kg of coconut shell porous carbon material was placed in a fluidized bed device, and 3 L / min of silane gas was introduced into the device. At a high temperature of 600 °C, silane was cracked to form elemental silicon, which was attached to the porous carbon pores and surface. The silane deposition time was 5 h. Then 3 L / min of acetylene gas was introduced into the device for carbon coating. The deposition time was 1 h. After cooling, the silicon-carbon precursor material was obtained.

[0046] (2) Take 1 kg of the silicon-carbon precursor material in step (1) to prepare a 20% by mass ratio silicon-carbon precursor material aqueous solution, then add 50 g of lithium dihydrogen phosphate and stir for 30 minutes to mix the solution evenly. Then, 30 g of lithium hydroxide is first prepared into a 20% lithium hydroxide aqueous solution, and then the lithium hydroxide solution is slowly added to the aforementioned silicon-carbon negative electrode solution to react lithium dihydrogen phosphate and lithium hydroxide to generate lithium phosphate, and the solution is stirred for 30 minutes to mix the components evenly.

[0047] (3) The solution in step (2) is filtered, and then the powder obtained by filtration is calcined at 600° C. for 2 h under argon atmosphere protection, and after cooling, a lithium phosphate-coated silicon-carbon negative electrode material is finally obtained.

[0048] The performance test method of the silicon-carbon negative electrode material is the same as that in Example 1, and the test results are shown in Table 1.

[0049] Example 4

[0050] (1) 1 kg of petroleum coke porous carbon material was placed in a fluidized bed device, and 3 L / min of silane gas was introduced into the device. At a high temperature of 600 °C, silane was cracked to form elemental silicon, which was attached to the porous carbon pores and surface. The silane deposition time was 5 hours. Then 3 L / min of acetylene gas was introduced into the device for carbon coating. The deposition time was 1 hour. After cooling, the silicon-carbon precursor material was obtained.

[0051] (2) Take 1 kg of the silicon-carbon precursor material in step (1) to prepare a 20% by mass ratio silicon-carbon precursor material aqueous solution, then add 50 g of sodium dihydrogen phosphate and stir for 30 minutes to mix the solution evenly. Then, 30 g of lithium hydroxide is first prepared into a 20% lithium hydroxide aqueous solution, and then the lithium hydroxide solution is slowly added to the aforementioned silicon-carbon negative electrode solution to react sodium dihydrogen phosphate and lithium hydroxide to generate lithium phosphate, and the solution is stirred for 30 minutes to mix the components evenly.

[0052] (3) The solution in step (2) is filtered, and then the powder obtained by filtration is calcined at 600° C. for 2 h under argon atmosphere protection, and after cooling, a lithium phosphate-coated silicon-carbon negative electrode material is finally obtained.

[0053] The performance test method of the silicon-carbon negative electrode material is the same as that in Example 1, and the test results are shown in Table 1.

[0054] Comparative Example 1

[0055] 1kg of coconut shell porous carbon material was placed in a fluidized bed device, and 3L / min of silane gas was introduced into the device. At a high temperature of 600°C, silane was cracked to form elemental silicon, which was attached to the porous carbon pores and surface. The silane deposition time was 5h. Then 3L / min of acetylene gas was introduced into the device for carbon coating. The deposition time was 1h, and the silicon-carbon negative electrode material was obtained after cooling.

[0056] The performance test method of the silicon-carbon negative electrode material is the same as that in Example 1, and the test results are shown in Table 1.

[0057] Table 1 Performance test results of silicon-carbon negative electrode materials ; It can be seen from the above table that the lithium phosphate-coated modified silicon-carbon negative electrode materials prepared in Examples 1 to 4 of the present invention have smaller specific surface areas than the silicon-carbon negative electrode material prepared in Comparative Example 1, which can reduce the contact opportunity between the electrolyte and the material surface, thereby inhibiting unnecessary side reactions, and can also simplify the production process and reduce the required time and energy consumption.

[0058] From the reversible capacity data, it can be seen that the prepared lithium phosphate coated modified silicon-carbon negative electrode material has good cycle stability; and the first discharge efficiency of the prepared lithium phosphate coated modified silicon-carbon negative electrode material is significantly higher than the silicon-carbon negative electrode material without lithium phosphate coating modification prepared in Comparative Document 1, indicating that the lithium phosphate coated modified silicon-carbon negative electrode material can effectively convert and release more energy, reduce the energy loss during the initial charge and discharge process, and improve the overall energy utilization efficiency of the battery.

[0059] The rate discharge retention rate of the silicon-carbon negative electrode material modified by lithium phosphate coating is significantly higher than that of the silicon-carbon negative electrode material without lithium phosphate coating, indicating that the silicon-carbon negative electrode material modified by lithium phosphate coating has excellent power performance, good electrical conductivity and stable electrode structure.

[0060] The 100-cycle cycle retention rate of the lithium phosphate coated and modified silicon-carbon negative electrode material is significantly higher than that of the silicon-carbon negative electrode material without lithium phosphate coating and modification, indicating that the lithium phosphate coated and modified silicon-carbon negative electrode material has good cycle stability and improves the durability of the battery.

[0061] The prepared high specific capacity lithium-ion battery negative electrode material not only significantly reduces the specific surface area of ​​the silicon-carbon negative electrode material, improves its rate and cycle stability, but also reduces the production cost and has good environmental friendliness.

[0062] Therefore, the present invention adopts the above-mentioned lithium phosphate-coated modified silicon-carbon negative electrode material and its preparation method to effectively solve the performance limitation problem of silicon-carbon negative electrode material in lithium-ion battery applications. The prepared high specific capacity lithium-ion battery negative electrode material not only significantly reduces the specific surface area of ​​the silicon-carbon negative electrode material, improves its rate and cycle stability, but also reduces the production cost, and has good environmental friendliness, and has broad application prospects and market competitiveness in the field of lithium-ion batteries.

[0063] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A lithium phosphate coated modified silicon-carbon negative electrode material, characterized in that: The silicon-carbon negative electrode material is a porous core-shell structure, including a silicon-carbon precursor material and a lithium phosphate coating layer coated on the outer layer of the silicon-carbon precursor material, wherein the silicon-carbon precursor material is composed of a porous carbon matrix and nano-silicon particles deposited in the pores and surface of the porous carbon matrix.

2. The lithium phosphate coated modified silicon-carbon negative electrode material according to claim 1, characterized in that: The diameter of the silicon-carbon negative electrode material is 1-20 μm, wherein silicon accounts for 30-60% of the silicon-carbon negative electrode material, carbon accounts for 30-60% of the silicon-carbon negative electrode material, and lithium phosphate accounts for 1-10% of the silicon-carbon negative electrode material.

3. A method for preparing a lithium phosphate coated modified silicon-carbon negative electrode material according to any one of claims 1 to 2, characterized in that: The following steps are involved: S1. Preparing silicon-carbon precursor material by CVD vapor deposition equipment; S2, performing liquid phase coating optimization on the silicon-carbon precursor material prepared in S1 to obtain a modified silicon-carbon material; S3. Treat the modified silicon-carbon material solution obtained in S2 to obtain a lithium phosphate-coated modified silicon-carbon negative electrode material.

4. The method for preparing a lithium phosphate-coated modified silicon-carbon negative electrode material according to claim 3, characterized in that: The specific operation of S1 is: placing the porous carbon material into a CVD vapor deposition device, introducing silane gas into the device, and under high temperature conditions, the silane in the device is cracked into silicon atoms and gradually deposited on the porous carbon material, while introducing a small amount of carbon source gas to deposit a thin carbon layer, and then cooling and discharging the material to form a silicon-carbon precursor material.

5. The method for preparing a lithium phosphate coated modified silicon-carbon negative electrode material according to claim 3, characterized in that: The specific operation of S2 is: dissolving the silicon-carbon precursor material obtained in S1 in a solvent and adding a phosphoric acid source, stirring the solution, adding a lithium hydroxide solution, allowing the phosphoric acid source and lithium hydroxide to react to generate lithium phosphate to coat the surface of the silicon-carbon precursor, thereby obtaining a modified silicon-carbon material.

6. The method for preparing a lithium phosphate coated modified silicon-carbon negative electrode material according to claim 3, characterized in that: The specific operation of S3 is: filtering the solution of the modified silicon-carbon material obtained in S2 to obtain a modified silicon-carbon mixed powder material, then calcining it under a high-temperature protective atmosphere, and obtaining a finished silicon-carbon material after cooling.

7. The method for preparing a lithium phosphate coated modified silicon-carbon negative electrode material according to claim 4, characterized in that: The specific operation of S3 is: filtering the solution of the modified silicon-carbon material obtained in S2 to obtain a modified silicon-carbon mixed powder material, and then drying it in a high-temperature drying oven at 80-120° C. for 1-3 hours, and obtaining a finished silicon-carbon material after cooling.

8. The method for preparing a lithium phosphate coated modified silicon-carbon negative electrode material according to claim 4, characterized in that: The CVD vapor deposition equipment in S1 is one or two of a rotary furnace and a fluidized bed. The deposition temperature of the silane and the carbon source in S1 is 500-800°C, the deposition time is 0.5-24h, the porous carbon-based material is one or more of coconut shell carbon, resin carbon, and petroleum coke, and the carbon source gas is one or more of methane, ethane, acetylene, and propylene.

9. The method for preparing a lithium phosphate coated modified silicon-carbon negative electrode material according to claim 5, characterized in that: The phosphate source in S2 is one or more of lithium dihydrogen phosphate, dilithium hydrogen phosphate, sodium dihydrogen phosphate and ammonium dihydrogen phosphate, and the solvent is one or both of water and ethanol.

10. The method for preparing a lithium phosphate coated modified silicon-carbon negative electrode material according to claim 6, characterized in that: The protective atmosphere in S3 is one or more of nitrogen, argon, and argon-hydrogen mixed gas. The calcination temperature is 500-800° C. and the calcination time is 0.5-24 h.

Citation Information

Patent Citations

  • Preparation method and product of lithium phosphate coated ternary ion battery positive electrode material

    CN109546136A

  • Preparation method of double-conducting-layer coated lithium-rich manganese-based material

    CN112510200A

  • Low-expansion silicon negative electrode material

    CN114792782A

  • Nano silicon-carbon composite material as well as preparation method and application thereof

    CN118173733A

Cited By

  • Double-layer coated silicon-carbon composite material, preparation method thereof and lithium ion battery

    CN119481021A

  • Method for preparing porous carbon structure containing sub-nanoscale ionic conduction improvement layer by using atomic layer deposition and application of porous carbon structure

    CN119695060A

  • Long-circulation silicon-carbon negative electrode material as well as preparation method and application thereof

    CN119725506A

  • Negative electrode material, preparation method thereof and lithium ion battery

    CN119994038A

  • High-energy silicon-carbon composite negative electrode material for lithium ion battery and preparation process of high-energy silicon-carbon composite negative electrode material

    CN120348941A