High-temperature-resistant low-loss nanocrystalline magnetism isolating material and preparation method thereof
By covering the nanocrystalline soft magnetic alloy strip with double-sided adhesive, crushing, composite and performing stress removal treatment of high-temperature heating, bending and winding, the problem of time-consuming existing processes is solved and the nanocrystalline magnetic isolation material is improved The preparation efficiency and performance stability are suitable for high-frequency communication equipment and other fields.
Patent Information
- Application Number
- CN202411040934.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
In the existing preparation process of high-temperature and low-loss nanocrystalline magnetic isolation materials, the high-temperature and high-humidity placement method consumes time and is low in efficiency, which affects the stability and reliability of electronic products.
Double-sided adhesive is applied to the nanocrystalline soft magnetic alloy strip, and the magnetic crushing and multi-layer composite is carried out, and then heated at 120-180℃ and bent and rolled. The stress treatment is removed through sharp corner fixtures and combined with edge wrapping treatment. , and obtain nanocrystal magnetic separator.
This method significantly shortens the stress removal time, improves the preparation efficiency, reduces eddy current loss, enhances the insulation effect, is suitable for large-scale production, and improves the thermal stability and performance stability of nanocrystalline magnetic isolation materials.
Smart Images

Figure CN118984580A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electromagnetic shielding and wireless charging magnetic sheet materials, and specifically relates to a high-temperature resistant and low-loss nanocrystalline magnetic isolation material and a preparation method thereof. Background Art
[0002] With the continuous advancement of science and technology, electronic products are gradually developing towards high frequency, miniaturization, and thinness. Product design is becoming more and more sophisticated and complex, and electromagnetic interference and heating problems are becoming more and more serious. In particular, some high-frequency applications have put forward higher requirements for product design. In addition to paying more attention to electromagnetic compatibility and heat dissipation design, it is also necessary to use advanced magnetic shielding materials to effectively reduce the impact of electromagnetic interference and ensure the stability and reliability of the product.
[0003] Nanocrystalline magnetic isolation sheet is a new type of material, usually made of nanocrystalline magnetic material. The microstructure of nanocrystalline material is very fine, the particle size is at the nanometer level, it has high saturation magnetic induction intensity and low coercivity, and can effectively absorb and shield external electromagnetic waves, providing electromagnetic isolation protection.
[0004] The magnetic isolation sheet itself will generate heat due to hysteresis loss, eddy current loss, magnetic loss and other reasons. A hot or high-temperature working environment will cause large fluctuations in the performance of the magnetic isolation shielding material, thereby affecting the stability of the performance of electronic products.
[0005] The development of high temperature resistant and low loss nanocrystalline magnetic isolation materials can greatly improve the stability and reliability of electronic products.
[0006] In the existing preparation process of high temperature resistant and low loss nanocrystalline magnetic isolation materials, a high temperature and high humidity placement method is used to remove stress, which is time-consuming and inefficient. Summary of the invention
[0007] Therefore, the technical problem to be solved by the present invention is to overcome the defects of the stress relief method in the prior art that it is time-consuming and inefficient, thereby providing a high-temperature resistant and low-loss nanocrystalline magnetic isolation material and a preparation method thereof.
[0008] To this end, the present invention provides the following technical solutions.
[0009] In a first aspect, the present invention provides a method for preparing a high temperature resistant and low loss nanocrystalline magnetic isolation material, comprising the following steps:
[0010] S1. Covering the nanocrystalline soft magnetic alloy strip with double-sided adhesive to obtain the adhesive-coated nanocrystalline strip;
[0011] S2, crushing the coated nanocrystalline strip to obtain a single-layer nanocrystalline magnetic layer;
[0012] S3, performing multi-layer composite on the single-layer nanocrystalline magnetic layer to obtain a composite material;
[0013] S4, performing stress relief treatment on the composite material to obtain a nanocrystalline magnetic isolation material;
[0014] The stress relief treatment includes: heating the composite material at 120-180°C, then bending it, and rolling it up under tension. For example, the composite material can be heated at 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, 150°C, 160°C, 170°C or 180°C, but is not limited to the listed values. Other values not listed in the numerical range are also applicable, preferably 130°C to 150°C.
[0015] Furthermore, the stress relief device used in the stress relief treatment includes a sharp-angle fixture, and the composite material is bent when passing through the sharp-angle fixture.
[0016] Furthermore, the top of the pointed-angle fixture is provided with a rounded corner with a radius R of 0.15 to 0.3 mm, and the angle α formed by the two side surfaces connected to the rounded corner is 85 to 95°; for example, R can be 0.15 mm, 0.20 mm, 0.25 mm or 0.3 mm, and α can be 85°, 90° or 95°, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0017] Furthermore, the feeding speed of the composite material is 3 to 8 m / min. For example, the feeding speed can be 3 m / min, 4 m / min, 5 m / min, 6 m / min, 7 m / min or 8 m / min, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable, and 3 to 5 m / min can be selected.
[0018] Furthermore, the stress relief device used in the stress relief treatment includes a material unwinding shaft, a material pressing shaft, a heating plate, a sharp angle fixture, a tension sensor and a material receiving shaft;
[0019] During the stress relief treatment process, the composite material passes through a press shaft, a heating plate, a sharp-angle fixture, a tension sensor, and a receiving shaft in sequence.
[0020] Furthermore, the tension applied during winding is 50-100N. For example, the tension may be 50N, 60N, 70N, 80N, 90N or 100N, but is not limited to the listed values. Other values not listed within the range are also applicable.
[0021] Furthermore, the method further includes S5, performing edge wrapping treatment on the composite material after the stress relief treatment.
[0022] Furthermore, the nanocrystalline soft magnetic alloy strip described in S1 is obtained by heat treating an amorphous soft magnetic alloy strip;
[0023] Optionally, the amorphous soft magnetic alloy strip is an iron-based amorphous soft magnetic alloy strip;
[0024] Optionally, the thickness of the amorphous soft magnetic alloy strip is 14 to 23um; for example, the thickness may be 14um, 15um, 16um, 17um, 18um, 19um, 20um, 21um, 22um or 23um, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] Optionally, the heat treatment includes heating from room temperature to a first temperature of 350-450°C, and keeping at the first temperature for 30-60 minutes; continuing to heat to a second temperature of 450-500°C, and keeping at the second temperature for 30-60 minutes; continuing to heat to a third temperature of 500-600°C, and keeping at the third temperature for 60-120 minutes. For example, the first temperature may be 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, 420°C or 450°C, and the holding time at the first temperature may be 30 min, 40 min, 50 min or 60 min; the second temperature may be 460°C, 470°C, 480°C, 490°C or 500°C, and the holding time at the second temperature may be 30 min, 40 min, 50 min or 60 min; the third temperature may be 500°C, 520°C, 540°C, 560°C, 580°C or 600°C, and the holding time at the third temperature may be 60 min, 70 min, 80 min, 90 min, 100 min, 110 min or 120 min, but it is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0026] Optionally, the heating rate from room temperature to the first temperature is 5 to 10° C. / min;
[0027] Optionally, the heating rate from the first temperature to the second temperature is 0.5 to 3°C / min;
[0028] Optionally, the heating rate from the second temperature to the third temperature is 1 to 3°C / min;
[0029] Preferably, the third temperature is 550-580°C;
[0030] Optionally, the heat treatment is carried out in a protective atmosphere, preferably, the protective atmosphere is nitrogen.
[0031] Furthermore, in S1, the double-sided adhesive tape comprises an adhesive layer, and the adhesive layer is selected from acrylic acid or acrylic acid modified by a dimethylsilane coupling agent;
[0032] Optionally, the adhesive layer thickness is 3 to 10 um;
[0033] Optionally, the double-sided adhesive further includes a substrate, and the substrate is polyimide.
[0034] Furthermore, in S2, the magnets are crushed by using a longitudinal and transverse bidirectional cross roller shearing method and / or by using an anilox roller with convex dots to roll and crush the magnets;
[0035] Optionally, the blade gap between the roller shears in the cross roller shear is 0.8 to 1.2 mm;
[0036] Optionally, the convex point size of the anilox roller is 0.8 to 1.2 mm;
[0037] Furthermore, in S3, a single-layer nanocrystalline magnetic layer is used to perform 2 to 5 layers of compounding to obtain a composite material.
[0038] Further, in S5, the upper and lower surfaces of the composite material after the stress relief treatment are edge-wrapped by laminating or die-cutting with an adhesive tape;
[0039] Optionally, the adhesive tape includes an adhesive layer, and the adhesive layer of the adhesive tape is acrylic acid modified by a dimethylsilane coupling agent;
[0040] Optionally, the adhesive tape further comprises a substrate, and the substrate of the adhesive tape is polyimide;
[0041] Optionally, the thickness of the tape is 0.01-0.1 mm.
[0042] In a second aspect, the present invention provides a high temperature resistant and low loss nanocrystalline magnetic isolation material prepared according to the preparation method.
[0043] The technical solution of the present invention has the following advantages:
[0044] 1. The preparation method of the high temperature resistant and low loss nanocrystalline magnetic insulation material of the present invention comprises the following steps: S1, coating a nanocrystalline soft magnetic alloy strip with double-sided tape to obtain a coated nanocrystalline strip; S2, crushing the coated nanocrystalline strip to obtain a single-layer nanocrystalline magnetic layer; S3, performing multi-layer composite processing on the single-layer nanocrystalline magnetic layer to obtain a composite material; S4, performing stress relief treatment on the composite material to obtain a nanocrystalline magnetic insulation material; the stress relief treatment comprises: heating the composite material at 120-180°C, then bending it, and rolling it up under tension.
[0045] The present invention creatively uses heating, bending and constant tension stretching to relieve stress, which takes less time and is more efficient than placing the stress under high temperature and high humidity.
[0046] Heating the composite material can release the stress generated when the crushed magnets are rolled and crushed into the nanocrystals during the crushing process. On the other hand, the double-sided adhesive is heated and has a certain fluidity at the microscopic level. When the composite material is bent, the gap between the fragments expands due to the force. After bending, the composite material shrinks and recovers, the gap narrows, and the adhesive layer of the double-sided adhesive partially penetrates into the gap. Rolling up under tension can increase the gap between the crushed magnet pieces, allowing the double-sided adhesive to better penetrate into the gap, so that both sides of the magnetic isolation sheet have an insulating adhesive layer, so as to obtain a magnetic isolation sheet with better insulation effect and reduce eddy current loss.
[0047] The preparation method of the high temperature resistant and low loss nanocrystalline magnetic isolation material of the present invention is simple and low in cost, and is suitable for large-scale production.
[0048] 2. The top of the sharp corner fixture is provided with a fillet with a radius R of 0.15 to 0.3 mm, and the angle α formed by the two side surfaces connected to the fillet is 85 to 95°. R is limited within the scope of this application, which can achieve a better stress relief effect while avoiding the sharp corner fixture from being too sharp, which may cause the sharp corner fixture to be easily worn, and also avoid the sharp corner fixture from scratching the composite material.
[0049] 3. The material feeding speed of the unwinding shaft is 3-8 m / min. The material feeding speed is limited within the scope of this application, which can ensure production efficiency while avoiding performance degradation caused by insufficient material heating.
[0050] 4. Edge wrapping of the composite material after stress relief treatment can enhance insulation, prevent edge particles from falling off, and prevent air / water vapor from entering the interior and affecting reliability.
[0051] 5. In S1, the double-sided adhesive tape includes an adhesive layer, and the adhesive layer is selected from acrylic acid or acrylic acid modified by a dimethylsilane coupling agent; optionally, the double-sided adhesive tape also includes a substrate, and the substrate is polyimide. The materials used for the adhesive layer and the substrate of the double-sided adhesive tape of the present invention can withstand temperatures of 120 to 180°C for a long time and can withstand temperatures of more than 200°C for a short time, so that the obtained nanocrystalline magnetic isolation material has more excellent thermal stability.
[0052] 6. The nanocrystalline magnetic isolation material prepared by the method of the present invention is suitable for high-frequency communication equipment, induction heating, radio equipment, antennas and other fields, and can improve signal transmission quality, reduce electromagnetic interference, and enhance equipment performance and stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0054] Figure 1 This is a schematic diagram of the structure of the single-sided coated nanocrystalline ribbon in Example 1;
[0055] Figure 2 This is a schematic diagram of the composite material structure in Example 1;
[0056] Figure 3 It is a schematic diagram of the structure of the stress relief device;
[0057] Figure 4 This is a schematic diagram of a sharp corner fixture;
[0058] Figure 5 This is a schematic diagram of the fillet of a sharp corner fixture;
[0059] Figure 6 Schematic diagram of composite material flow during stress relief process;
[0060] Figure 7 It is a schematic diagram of the three-dimensional structure of the stress relief device;
[0061] Figure 8 Schematic diagram of the structure of the nanocrystalline magnetic isolation material prepared in Example 1.
[0062] Reference numerals:
[0063] 1- unloading shaft; 2- pressing shaft; 3- heating plate; 4- sharp corner fixture; 5- tension sensor; 6- receiving shaft. DETAILED DESCRIPTION
[0064] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0065] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0066] Example 1
[0067] This embodiment provides a method for preparing a high temperature resistant and low loss nanocrystalline magnetic isolation material, comprising the following steps:
[0068] (1) An iron-based amorphous soft magnetic alloy strip with a thickness of 20 μm was heat treated in a nitrogen protective atmosphere: the temperature was raised from room temperature to 400°C for 60 min and kept at this temperature for 30 min; the temperature was raised from 400°C to 450°C for 60 min and kept at this temperature for 40 min; the temperature was raised from 450°C to 565°C for 60 min and kept at this temperature for 120 min before being cooled in the furnace to obtain an iron-based nanocrystalline soft magnetic alloy strip with a thickness of 20 μm.
[0069] (2) The iron-based nanocrystalline soft magnetic alloy strip obtained in step (1) is coated on one side with a substrate-free double-sided adhesive with a thickness of 3 μm (the double-sided adhesive has a PET film for process protection, which needs to be removed during the subsequent step (4) of lamination), and the adhesive layer of the substrate-free double-sided adhesive is an acrylic adhesive (Furukawa, FT N003); the other side is a bare surface, and the following is obtained: Figure 1 Single-sided coated nanocrystalline ribbon shown.
[0070] (3) The single-sided coated nanocrystalline strip obtained in step (2) is crushed by longitudinal and transverse cross-roll shearing and fine mesh roller with raised dots, wherein the blade gap between the cross-roll shears is 1.0 mm, and the raised dot size of the fine mesh roller is 0.8 mm, to obtain a single-layer nanocrystalline magnetic layer, and the size of the fine flakes separated by microcracks in the fragment unit is about 0.05 mm.
[0071] (4) Compounding the single-layer nanocrystalline magnetic layer obtained in step (3) into three layers, and attaching a layer of double-sided adhesive to the bare surface of the composite laminated structure to obtain a composite material with a thickness of 72 μm, such as Figure 2 shown.
[0072] (5) The composite material obtained in step (4) is used Figure 3-Figure 7 The stress relief device shown is used for heating, bending and winding. The stress relief device includes a discharge shaft 1, a pressing shaft 2, a heating plate 3, a sharp corner fixture 4, a tension sensor 5 and a winding shaft 6; during the stress relief treatment, the composite material is placed on the discharge shaft 1, and passes through the pressing shaft 2, the heating plate 3, the sharp corner fixture 4, the tension sensor 5, and the winding shaft 6 in sequence. The heating plate 3 is a cast aluminum heating plate. The temperature of the heating plate 3 is set at 150°C, the length of the heating plate 3 is 400mm, the feeding speed of the composite material is 5m / min, the top corner radius of the sharp corner fixture 4 is R=0.15mm, the angle α of the sharp corner fixture is 90°, and the winding tension is 90N.
[0073] (6) The upper and lower surfaces of the composite material after stress relief in step (5) are edge-wrapped by bonding with adhesive tape to obtain a Figure 8 The nanocrystalline magnetic isolation material shown in the figure. The adhesive tape comprises a PI substrate and an acrylic acid (Furukawa, N003T) adhesive layer modified by a bismethylsilane coupling agent coated on the substrate, and the thickness of the adhesive tape is 0.01 mm.
[0074] Example 2
[0075] This embodiment provides a method for preparing a high-temperature resistant and low-loss nanocrystalline magnetic shielding material. The preparation process is basically the same as that of Example 1, except that the temperature of the heating plate is set at 150°C, the feed speed of the composite material is 5m / min, the sharp-angle fixture R=0.25mm, and the winding tension is 90N.
[0076] Example 3
[0077] This embodiment provides a method for preparing a high-temperature resistant and low-loss nanocrystalline magnetic shielding material. The preparation process is basically the same as that of Example 1, except that the temperature of the heating plate is set at 150°C, the feed speed of the composite material is 5m / min, the sharp-angle fixture R=0.15mm, and the winding tension is 60N.
[0078] Example 4
[0079] This embodiment provides a method for preparing a high-temperature resistant and low-loss nanocrystalline magnetic shielding material. The preparation process is basically the same as that of Example 1, except that the temperature of the heating plate is set at 120°C, the feed speed of the composite material is 5m / min, the sharp-angle fixture R=0.15mm, and the winding tension is 90N.
[0080] Example 5
[0081] This embodiment provides a method for preparing a high-temperature resistant and low-loss nanocrystalline magnetic shielding material. The preparation process is basically the same as that of Example 1, except that the temperature of the heating plate is set at 180°C, the feed speed of the composite material is 5m / min, the sharp-angle fixture R=0.15mm, and the winding tension is 90N.
[0082] Example 6
[0083] This embodiment provides a method for preparing a high-temperature resistant and low-loss nanocrystalline magnetic shielding material. The preparation process is basically the same as that of Example 1, except that the temperature of the heating plate is set at 150°C, the feed speed of the composite material is 3m / min, the sharp-angle fixture R=0.15mm, and the winding tension is 90N.
[0084] Example 7
[0085] This embodiment provides a method for preparing a high-temperature resistant and low-loss nanocrystalline magnetic shielding material. The preparation process is basically the same as that of Example 1, except that the temperature of the heating plate is set at 150°C, the feed speed of the composite material is 8m / min, the sharp-angle fixture R=0.15mm, and the winding tension is 90N.
[0086] Comparative Example 1
[0087] This comparative example provides a method for preparing a nanocrystalline magnetic shielding material. The preparation process is basically the same as that of Example 1, except that step (5) is not performed.
[0088] Test example
[0089] The composite materials obtained in steps (1) to (4) of the embodiments and comparative examples are directly hemmed according to step (6), and the obtained samples are used as samples for testing the properties before heating and stretching.
[0090] The nanocrystalline magnetic insulation materials prepared according to the steps of various embodiments and comparative examples are used as samples to test the performance after heating and stretching.
[0091] The nanocrystalline magnetic isolation materials prepared according to the steps of the embodiments and comparative examples were left to stand at room temperature for 24 hours to serve as samples for testing the performance of the materials after standing for 24 hours.
[0092] The nanocrystalline magnetic insulation materials prepared according to the steps of the embodiments and comparative examples were baked at 120° C. for 24 hours and then cooled to serve as samples for testing the performance after being baked at 120° C. for 24 hours and then cooled.
[0093] The magnetic permeability u' and imaginary magnetic permeability u" were tested at frequencies of 128KHz and 6.78MHz before heating and stretching, after heating and stretching, after standing for 24 hours, after baking at high temperature of 120℃ for 24 hours and after cooling.
[0094] The test equipment is Agilent E4990A impedance analyzer. The test results are shown in Table 1 and Table 2.
[0095] Table 1 Magnetic performance parameters of magnetic shielding materials at 128KHz
[0096]
[0097] Table 2 Magnetic performance parameters of magnetic shielding materials at 6.78MHz
[0098]
[0099] It can be seen from Table 2 that after the stress relief treatment of the present invention, the magnetic permeability u' and the imaginary magnetic permeability u" are reduced, and the obtained magnetic shielding materials all meet u'=220-300, u"<100 at a frequency of 6.78 MHz, and the loss is significantly reduced.
[0100] It can be seen from Table 1 and Table 2 that after the stress relief treatment of the present invention, the stability of material performance is significantly improved, and the range of change at room temperature or high temperature is very small.
[0101] From the comparison between Example 1 and Example 2, it can be seen that when the radius of the top corner of the sharp-angle fixture is 0.15 mm, u" is lower, the change rate of u' and u" is smaller, and the stability is better.
[0102] From the comparison among Example 1, Example 4 and Example 5, it can be seen that when the heating temperature is lowered, the material properties will decrease; when the temperature is increased, the material properties will be improved to a certain extent, but not significantly. Considering the production safety, the preferred temperature is 150°C.
[0103] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.
Claims
1. A method for preparing a high temperature resistant and low loss nanocrystalline magnetic isolation material, characterized in that: The following steps are involved: S1. Covering the nanocrystalline soft magnetic alloy strip with double-sided adhesive to obtain the adhesive-coated nanocrystalline strip; S2, crushing the coated nanocrystalline strip to obtain a single-layer nanocrystalline magnetic layer; S3, performing multi-layer composite on the single-layer nanocrystalline magnetic layer to obtain a composite material; S4, performing stress relief treatment on the composite material to obtain a nanocrystalline magnetic isolation material; The stress relief treatment comprises: heating the composite material at 120-180° C., then bending it, and rolling it up under tension.
2. The method for preparing the high temperature resistant and low loss nanocrystalline magnetic isolation material according to claim 1, characterized in that: The stress relief device used in the stress relief treatment includes a sharp-angle fixture, and the composite material is bent when passing through the sharp-angle fixture.
3. The method for preparing the high temperature resistant and low loss nanocrystalline magnetic isolation material according to claim 2, characterized in that: The top of the sharp-angle fixture is provided with a fillet with a radius R of 0.15 to 0.3 mm, and the angle α formed by the two side surfaces connected to the fillet is 85 to 95°; and / or The material feeding speed of the composite material is 3-8 m / min, and can be optionally 3-5 m / min.
4. The method for preparing the high temperature resistant and low loss nanocrystalline magnetic isolation material according to any one of claims 1 to 3, characterized in that: The tension applied during winding is 50~100N.
5. The method for preparing the high temperature resistant and low loss nanocrystalline magnetic isolation material according to any one of claims 1 to 3, characterized in that: The method also includes S5, performing edge wrapping treatment on the composite material after the stress relief treatment.
6. The method for preparing the high temperature resistant and low loss nanocrystalline magnetic isolation material according to any one of claims 1 to 3, characterized in that: The nanocrystalline soft magnetic alloy strip described in S1 is obtained by heat treating an amorphous soft magnetic alloy strip; Optionally, the amorphous soft magnetic alloy strip is an iron-based amorphous soft magnetic alloy strip; Optionally, the thickness of the amorphous soft magnetic alloy strip is 14 to 23 um; Optionally, the heat treatment condition is 500-600°C for 60-120 min; preferably, the heat treatment temperature is 550-580°C; Optionally, the heat treatment is carried out in a protective atmosphere, preferably, the protective atmosphere is nitrogen.
7. The method for preparing a high temperature resistant and low loss nanocrystalline magnetic isolation material according to any one of claims 1 to 3, characterized in that: In S1, the double-sided adhesive tape comprises an adhesive layer, and the adhesive layer is selected from acrylic acid or acrylic acid modified by a dimethylsilane coupling agent; Optionally, the adhesive layer thickness is 3 to 10 um; Optionally, the double-sided adhesive further includes a substrate, and the substrate is polyimide.
8. The method for preparing a high temperature resistant and low loss nanocrystalline magnetic isolation material according to any one of claims 1 to 3, characterized in that: At least one of the following conditions is met: (1) In S2, the magnets are crushed by using a longitudinal and transverse bidirectional cross roller shearing method and / or by using an anilox roller with convex dots to roll and crush the magnets; Optionally, the blade gap between the roller shears in the cross roller shear is 0.8 to 1.2 mm; Optionally, the convex point size of the anilox roller is 0.8 to 1.2 mm; (2) In S3, a single nanocrystalline magnetic layer is used to compound 2 to 5 layers to obtain a composite material.
9. The method for preparing the high temperature resistant and low loss nanocrystalline magnetic isolation material according to claim 5, characterized in that: In S5, the upper and lower surfaces of the composite material after stress relief treatment are edge-wrapped by laminating or die-cutting with adhesive tape; Optionally, the adhesive tape includes an adhesive layer, and the adhesive layer of the adhesive tape is acrylic acid modified by a dimethylsilane coupling agent; Optionally, the adhesive tape further comprises a substrate, and the substrate of the adhesive tape is polyimide; Optionally, the thickness of the tape is 0.01-0.1 mm.
10. A high temperature resistant and low loss nanocrystalline magnetic isolation material, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 9.
Citation Information
Cited By
Preparation method of short-process nanocrystalline magnetism isolating material
CN119446701A