Preparation method of multifunctional full-biomass aerogel with photothermal conversion capability
By combining cellulose nanofibers, hydroxyapatite nanowires and cuttlefish meal, a multifunctional full biomass aerogel with photothermal conversion capabilities was prepared, which solved the problems of insufficient material performance and complex preparation in the prior art. It achieves efficient seawater desalination, wastewater treatment and oil-water separation, and has excellent photothermal conversion and mechanical stability.
Patent Information
- Application Number
- CN202410994391.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-24
AI Technical Summary
The existing aerogel materials have shortcomings in light absorption, photothermal conversion capacity, water transmission capacity and elastic properties. The preparation process is complex and costly, which limits its wide range of seawater desalination, sewage treatment and solar steam power generation. application.
Using cellulose nanofibers, hydroxyapatite nanowires and cuttlefish meal as main components, they form a uniform slurry and freeze-dry them by stirring to prepare a multifunctional full biomass aerogel with photothermal conversion ability, and the material is hydrophilic. Good, excellent photothermal conversion efficiency and mechanical stability.
Aerogel preparation with low cost and simple process is achieved, the light energy utilization rate and evaporation efficiency is improved, and it has excellent water transmission performance and mechanical stability. It is suitable for seawater desalination, wastewater treatment and oil-water separation, and is environmentally friendly and non-toxic. .
Smart Images

Figure CN118988178A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of materials, relates to water treatment biomass aerogel, and specifically relates to a preparation method of a multifunctional all-biomass aerogel with light-heat conversion capability. Background Art
[0002] Water is the most important natural resource on earth and is closely related to human living environment and society. Three quarters of the earth's total area is covered by water, but seawater accounts for 97.5% and freshwater resources account for only 2.5%. The rapid growth of industrialization and population has led to serious water pollution and shortage of freshwater resources. Water pollution and shortage of freshwater resources have made the extraction of clean fresh water from abundant seawater and the treatment of sewage a hot topic. The sources of water pollution include domestic wastewater, factory pollution, fertilizer use, heavy metal wastewater, pharmaceutical waste liquid, etc.
[0003] Desalination and sewage treatment are currently the best ways to solve the problem of insufficient water resources and poor water quality. However, existing aerogel materials have many problems such as low light absorption, poor photothermal conversion ability, insufficient water transmission capacity, and poor elastic properties. Ming et al. cleverly assembled 3D porous macroscopic aerogels into a whole through a graphene oxide (GO)-assisted process using 2D Ti3C2Tx (MXene) as an independent solar-driven interfacial evaporator (GMA) to achieve efficient and all-round water purification. (Carbon, 2020, 167, 85-295) Noureen et al. loaded Ag3VO4 nanoparticles on a reduced graphene oxide carrier, which has the remarkable characteristics of large specific surface area, high porosity and surface roughness. The aerogel is prepared in a simple way and can be used in solar steam power generation, photocatalytic degradation / disinfection of organic pollutants and integrated water purification systems for desalination. (Nano Today, 2024, 54, 102130). Wang et al. prepared a MXene-based composite aerogel with interconnected porous structure, wide and high solar absorption, good wettability and photothermal performance. The aerogel was rationally designed in terms of structure and composition, which reduced the evaporation heat of water. The solar steam generator based on the aerogel showed a high energy density of 2.31 kg / m under one solar radiation. -2 h -1 The excellent water vapor evaporation rate of the aerogel also has good adsorption capacity to remove heavy metal ions from water, as well as good antibacterial ability, which should be helpful for solar steam generators to handle complex working environments. The above methods for preparing aerogel materials have problems such as expensive materials and cumbersome preparation processes, which are not conducive to large-scale preparation. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention aims to provide a method for preparing a multifunctional all-biomass aerogel with photothermal conversion capability, which has a simple preparation process, low cost and can be applied on a large scale.
[0005] The present invention is achieved through the following technical solutions:
[0006] A method for preparing a multifunctional all-biomass aerogel with photothermal conversion capability comprises dissolving cellulose nanofibers and hydroxyapatite nanowires in an alkaline solution and stirring to form a uniform slurry, then adding cuttlefish powder and a cross-linking agent and stirring to form a uniform slurry, freezing the slurry in a refrigerator, and then freeze-drying the slurry to obtain a multifunctional all-biomass aerogel with photothermal conversion capability; wherein the mass ratio of the cellulose nanofibers, the hydroxyapatite nanowires and the cuttlefish powder is (3-4):(1-2):(1-3), and the mass ratio of the alkaline solution to the cellulose nanofibers is (90-2):1.
[0007] Furthermore, the alkaline solution is sodium hydroxide and / or potassium hydroxide.
[0008] Furthermore, the cross-linking agent is epichlorohydrin and / or glutaraldehyde.
[0009] Furthermore, the freezing time is 2 to 10 hours, and the freeze-drying time is 24 to 48 hours.
[0010] Furthermore, the cellulose nanofiber and hydroxyapatite nanowire solution is stirred for 18 to 24 hours.
[0011] Furthermore, the cellulose nanofibers are prepared by the following method:
[0012] The raw material containing cellulose is dried, and lignin is removed and extracted using an inorganic solution in a heated oil bath magnetic stirrer. After drying, the raw material is crushed using a crusher to obtain cellulose nanofibers.
[0013] Furthermore, the raw materials containing cellulose are crop straw, flax, cotton, industrial hemp and wood; the raw materials are placed in a vertical air drying oven, the temperature of the oven is 60-100° C., and the drying time is 24-48 hours.
[0014] Furthermore, the inorganic solvent for removing lignin is a mixture of one or more of sodium chlorite, acetic acid and propionic acid; the concentration of the inorganic solution for removing lignin is 0.005-3.0 g / mL, and the mass ratio of the inorganic solution for removing lignin to the dried cellulose-containing raw material is (50-300):1;
[0015] The solvent for extracting cellulose nanofibers is a mixture of sodium hydroxide, potassium hydroxide or one or more thereof; the concentration of the cellulose nanofiber extraction solution is 0.005-3.0 g / mL, and the mass ratio of the cellulose extraction solution to the extracted cellulose is (50-300):1.
[0016] Furthermore, the insulation temperature of the heating oil bath magnetic stirrer is 50 to 200° C., and the insulation time is 4 to 20 hours.
[0017] Furthermore, the hydroxyapatite nanowires are prepared by the following method: 10 mL of a 0.05 g / mL sodium hydroxide solution, 10 mL of a 0.0176 g / mL calcium chloride solution and 10 mL of anhydrous sodium dihydrogen phosphate solution with a concentration of 0.023 g / mL are sequentially added dropwise to 7.128 g of oleic acid and 9 mL of anhydrous ethanol, stirred, subjected to hydrothermal reaction for 12-24 h, and dried in a vertical forced air drying oven at 180° C. for 24 h to obtain hydroxyapatite nanowires.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The invention discloses a method for preparing a multifunctional all-biomass aerogel with photothermal conversion capability. Cellulose nanofibers and hydroxyapatite nanowires are mixed and stirred and a cross-linking agent is added. Finally, cuttlefish powder is added to improve the absorbance. Finally, the three are mixed and freeze-dried to obtain a multifunctional all-biomass aerogel with photothermal conversion capability. It has the advantages of simple preparation process, low cost and large-scale application. The aerogel with hydrophilic cellulose nanofibers and hydroxyapatite nanowires as the matrix has good hydrophilicity, natural water transmission channels, and provides a favorable way for water transmission, and has excellent water supply capacity. As an interfacial solar thermal aerogel, it greatly reduces the loss of heat. As a photothermal material, cuttlefish powder has good light absorption capacity and photothermal conversion capacity, improves the utilization rate of light energy, and improves the evaporation efficiency. The three-dimensional network structure provides a favorable channel for water transmission and water escape.
[0020] The three-dimensional network structure of the aerogel prepared by the present invention can increase the refraction of light, have excellent light-to-heat conversion efficiency, enhance the light absorption capacity and utilization rate, and avoid energy waste. By using clean and green solar energy, efficient solar energy interface evaporation is achieved, and seawater desalination, wastewater treatment, organic dye and oil-water separation treatment are accelerated.
[0021] The aerogel has excellent underwater superoleophobic properties, which can eliminate the impact of oil on the surface. More importantly, the aerogel has excellent mechanical stability. After continuous compression, its plastic deformation is almost zero, and it maintains excellent evaporation performance.
[0022] The aerogel prepared by the present invention has excellent light-to-heat conversion efficiency, excellent mechanical stability and chemical stability, low cost, simple preparation process, and the materials used are all biomass materials. It is environmentally friendly, has no secondary pollution, is non-toxic and harmless, and has a simple preparation process. It has broad application prospects in seawater desalination, wastewater treatment, organic dye liquor treatment and oil-water separation. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The aerogel prepared by the present invention is shown in the studio state and the highest surface temperature.
[0024] Figure 2 is a mass curve of water loss of aerogel prepared by the present invention under 1 sun;
[0025] FIG3( a ) is a curve of applying and releasing external force and a physical picture of the aerogel prepared by the present invention;
[0026] FIG3( b ) is a schematic diagram of plastic deformation of the aerogel glue prepared by the present invention after continuous and repeated compression for 5000 times;
[0027] Figure 4 It is a schematic diagram of the treatment of water in organic dyes by the aerogel prepared by the present invention;
[0028] (a) is a light absorption waveform of methylene blue solution before and after evaporation; (b) is a light absorption waveform of rhodamine B solution before and after evaporation;
[0029] Figure 5 This is a schematic diagram of the aerogel prepared by the present invention in oil-water separation;
[0030] Figure 6 Schematic diagram of the self-desalting performance of the aerogel prepared by the present invention;
[0031] Figure 7 is a flow chart of aerogel preparation of the present invention;
[0032] Figure 8 It is a schematic diagram of the working mechanism of the aerogel prepared by the present invention. DETAILED DESCRIPTION
[0033] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0034] The present invention discloses a method for preparing a multifunctional all-biomass aerogel with light-heat conversion capability, and the preparation method specifically comprises the following steps:
[0035] Step 1, drying the raw material containing cellulose, removing and extracting lignin with an inorganic solution in a heated oil bath magnetic stirrer, freeze-drying, and then crushing with a crusher to obtain cellulose nanofibers;
[0036] Step 2, 10 mL of sodium hydroxide solution, 10 mL of calcium chloride solution and 10 mL of anhydrous sodium dihydrogen phosphate solution are added dropwise to the prepared oleic acid and ethanol solution in sequence, stirred, hydrothermally reacted for 12-24 hours, and freeze-dried to obtain hydroxyapatite nanowires;
[0037] Step 3, dissolving the obtained cellulose nanofibers and hydroxyapatite nanowires in water, stirring to form a uniform slurry, adding cuttlefish powder, adding a cross-linking agent, and placing in a refrigerator;
[0038] Step 4: After freeze drying, a multifunctional all-biomass aerogel with photothermal conversion capability is obtained.
[0039] (1) The raw material of cellulose nanofiber is placed in a vertical air drying oven, the temperature of the vertical air drying oven is 60-100°C, and the drying time is 24-48h. The dried cellulose raw material is placed in a lignin removal inorganic solution with a concentration of 0.005-3.0g / mL, the mass ratio of the lignin removal inorganic solution to the dried cellulose-containing raw material is 50:1-300:1, and the temperature of the heated oil bath magnetic stirrer is 50-200°C for 4-20h; then cellulose is extracted, the concentration of the extracted cellulose nanofiber solution is 0.005-3.0g / mL, the mass ratio of the cellulose extraction solution to the extracted cellulose is 50:1-300:1, the temperature of the heated oil bath magnetic stirrer is 60°C, the insulation time is 4h, and the freeze-drying time is 24-48h. Among them, the raw material of cellulose nanofiber comes from crop straw, flax, cotton, industrial hemp and wood, but is not limited to these. The inorganic solvent for removing lignin is a mixture of sodium chlorite, acetic acid and propionic acid or one or more thereof. The solvent for extracting cellulose nanofibers is a mixture of sodium hydroxide and potassium hydroxide or one or more thereof.
[0040] (2) 10 mL of sodium hydroxide solution, 10 mL of calcium chloride solution and 10 mL of anhydrous sodium dihydrogen phosphate solution are added dropwise to the prepared oleic acid and ethanol solutions in sequence, and stirred. The mixture is hydrothermally reacted for 12-24 hours, and freeze-dried to obtain hydroxyapatite nanowires.
[0041] (3) Dissolving the extracted cellulose nanofibers and hydroxyapatite nanowires in an alkaline solution with a concentration of 0.01 to 2.0 g / mL, wherein the mass ratio of the solution for dissolving the cellulose nanofibers and hydroxyapatite nanowires to the cellulose is 90:1 to 2:1, and the mass ratio of the crosslinking agent to the solution is 1:24 to 1:6. A uniform slurry is obtained. The inorganic substance added to the dissolving agent is a mixture of one or more KOH and NaOH. The crosslinking agent for the cellulose nanofibers and hydroxyapatite nanowires is a mixture of one or more epichlorohydrin and glutaraldehyde.
[0042] (4) The obtained uniform slurry is frozen for 2-10 hours and then freeze-dried, wherein the freeze-drying time is 24-48 hours, and finally a multifunctional all-biomass aerogel with photothermal conversion capability is obtained.
[0043] Example 1
[0044]
[0045]
[0046] The cellulose raw material was placed in an oven for drying at a temperature of 60°C for 24 hours. The mass of the cellulose raw material was 30 g. The dried cellulose raw material was added to a sodium chlorite solution with a concentration of 0.02 g / mL and 2 mL of acetic acid. The temperature was kept at 90°C in a heating oil bath magnetic stirrer for 8 hours. After removing lignin, cellulose was subsequently extracted. The lignin-removed raw material was added to a NaOH solution with a concentration of 0.05 g / mL. The temperature of the heating oil bath magnetic stirrer was 60°C for 4 hours and freeze-dried for 24 hours.
[0047] 7.128g of oleic acid, 9mL of anhydrous ethanol, 0.05g / mL of sodium hydroxide solution, 0.0176g / mL of calcium chloride solution, and 0.023g / mL of anhydrous sodium dihydrogen phosphate were added dropwise in 10mL order, the temperature of the vertical forced air drying oven was 180°C, and the reaction time was 24h. Cellulose nanofibers and hydroxyapatite nanowires were dissolved in a NaOH solution (25mL) with a concentration of 0.1g / mL, stirred for 18h, 2mL of glutaraldehyde was added, and then 0.3g of cuttlefish powder was added, frozen for 5h, and freeze-dried for 48h to obtain a multifunctional all-biomass aerogel with photothermal conversion capability. Figure 1 As shown in the figure, under the light intensity of 1 sun, the surface temperature of the hydrogel quickly rises to 41.9°C, which has good photothermal conversion ability.
[0048] Example 2
[0049]
[0050] The cellulose raw material was placed in an oven for drying at 80°C for 36 hours. The mass of the cellulose raw material was 30 g. The dried cellulose raw material was added to a sodium chlorite solution with a concentration of 0.1 g / mL and 2 mL of acetic acid. The temperature was kept at 120°C for 6 hours in a heated oil bath magnetic stirrer. After removing lignin, cellulose was subsequently extracted. The lignin-removed raw material was added to a NaOH solution with a concentration of 0.1 g / mL. The temperature of the heated oil bath magnetic stirrer was 60°C for 4 hours and freeze-dried for 30 hours.
[0051] 7.128g of oleic acid, 9mL of anhydrous ethanol, 0.05g / mL of sodium hydroxide solution, 0.0176g / mL of calcium chloride solution, and 0.023g / mL of anhydrous sodium dihydrogen phosphate were added dropwise in 10mL order. The temperature of the vertical forced air drying oven was 180°C and the reaction time was 24h. Cellulose nanofibers and hydroxyapatite nanowires were dissolved in a KOH solution (25mL) with a concentration of 0.6g / mL, stirred for 20h, 2mL of epichlorohydrin was added, and then 0.1g of cuttlefish powder was added. The mixture was frozen for 7h and freeze-dried for 30h to obtain a multifunctional all-biomass aerogel with photothermal conversion capability. Figure 2 As shown in Figure 2, under a 1-sun light intensity, the water evaporation of the hydrogel in one hour reaches 1.92 kg m -2 .
[0052] Example 3
[0053]
[0054]
[0055] The cellulose raw material was placed in an oven for drying at a temperature of 100°C for 24 hours. The mass of the cellulose raw material was 30 g. The dried cellulose raw material was added to a sodium chlorite solution with a concentration of 3.0 g / mL and 2 mL of propionic acid. The temperature was kept at 60°C in a heating oil bath magnetic stirrer for 12 hours. After removing lignin, cellulose was subsequently extracted. The lignin-removed raw material was added to a NaOH solution with a concentration of 3.0 g / mL. The temperature of the oil bath magnetic stirrer was heated to 60°C for 4 hours and freeze-dried for 48 hours.
[0056] 7.128g of oleic acid, 9mL of anhydrous ethanol, 0.05g / mL of sodium hydroxide solution, 0.0176g / mL of calcium chloride solution, and 0.023g / mL of anhydrous sodium dihydrogen phosphate were added dropwise in 10mL, the temperature of the vertical air drying oven was 180℃, and the reaction time was 24h. Cellulose nanofibers and hydroxyapatite nanowires were dissolved in a NaOH solution (25mL) with a solution concentration of 0.5g / mL, stirred for 18h, 2mL of epichlorohydrin was added, and then 0.1g of cuttlefish powder was added, frozen for 3h, freeze-dried for 40h, and a multifunctional all-biomass aerogel with photothermal conversion capability was obtained. As shown in Figure 3(a) and Figure 3(b), when compressed underwater to 80% deformation, the maximum pressure reached 15.2kPa, and after 5000 cycles of compression, there was almost no plastic deformation.
[0057] Example 4
[0058]
[0059]
[0060] The cellulose raw material was placed in an oven for drying at a temperature of 60°C for 36 hours. The mass of the cellulose raw material was 30 g. The dried cellulose raw material was added to a sodium chlorite solution with a concentration of 0.5 g / mL and 2 mL of acetic acid. The temperature was kept at 150°C for 4 hours in a heating oil bath magnetic stirrer. After removing lignin, cellulose was subsequently extracted. The lignin-removed raw material was added to a NaOH solution with a concentration of 0.005 g / mL, the temperature of the oil bath magnetic stirrer was heated to 60°C, the temperature was kept for 4 hours, and freeze-dried for 30 hours.
[0061] 7.128g of oleic acid, 9mL of anhydrous ethanol, 0.05g / mL of sodium hydroxide solution, 0.0176g / mL of calcium chloride solution, and 0.023g / mL of anhydrous sodium dihydrogen phosphate were added dropwise in 10mL order, the temperature of the vertical forced air drying oven was 180°C, and the reaction time was 18h. Cellulose nanofibers and hydroxyapatite nanowires were dissolved in a NaOH solution (25mL) with a concentration of 0.06g / mL, stirred for 24h, 2mL of epichlorohydrin was added, and then 0.2g of cuttlefish powder was added, frozen for 8h, and freeze-dried for 24h to obtain a multifunctional all-biomass aerogel with photothermal conversion capability. Figure 4 As shown, the UV spectrophotometer and physical images of the organic dye solution (methylene blue and rhodamine B) and the condensed water obtained after evaporation prove that the pollution of organic dyes can be removed.
[0062] Example 5
[0063]
[0064] The cellulose raw material was placed in an oven for drying at 80°C for 36 hours. The mass of the cellulose raw material was 30 g. The dried cellulose raw material was added to a sodium chlorite solution with a concentration of 0.5 g / mL and 2 mL of acetic acid. The temperature was kept at 100°C for 6 hours in a heating oil bath magnetic stirrer. After removing lignin, cellulose was subsequently extracted. The lignin-removed raw material was added to a KOH solution with a concentration of 0.05 g / mL. The temperature of the heating oil bath magnetic stirrer was 60°C for 4 hours and freeze-dried for 36 hours.
[0065] 7.128g of oleic acid, 9mL of anhydrous ethanol, 0.05g / mL of sodium hydroxide solution, 0.0176g / mL of calcium chloride solution, and 0.023g / mL of anhydrous sodium dihydrogen phosphate were added dropwise in 10mL order, the temperature of the vertical forced air drying oven was 180°C, and the reaction time was 24h. Cellulose nanofibers and hydroxyapatite nanowires were dissolved in a NaOH solution (25mL) with a concentration of 0.032g / mL, stirred for 20h, 2mL of epichlorohydrin was added, and then 0.3g of cuttlefish powder was added, frozen for 5h, and freeze-dried for 36h to obtain a multifunctional all-biomass aerogel with photothermal conversion capability. Figure 5 As shown, it has a good separation effect on oil-water mixture.
[0066] Example 6
[0067]
[0068]
[0069] like Figure 7 As shown, the cellulose raw material is placed in an oven for drying, the oven temperature is 80°C, and the drying time is 24h. The mass of the cellulose raw material is 30g, and the dried cellulose raw material is added to a sodium chlorite solution with a concentration of 0.1g / mL and 2mL of acetic acid, and the temperature of the heated oil bath magnetic stirrer is kept at 150°C for 8h. After removing lignin, cellulose is subsequently extracted, and the lignin-removed raw material is added to a NaOH solution with a concentration of 0.08g / mL, and the temperature of the heated oil bath magnetic stirrer is 60°C, and the temperature is kept for 4h, and freeze-dried for 24h.
[0070] 7.128g of oleic acid, 9mL of anhydrous ethanol, 0.05g / mL of sodium hydroxide solution, 0.0176g / mL of calcium chloride solution, and 0.023g / mL of anhydrous sodium dihydrogen phosphate were added dropwise in 10mL order. The temperature of the vertical forced air drying oven was 180°C and the reaction time was 24h. Cellulose nanofibers and hydroxyapatite nanowires were dissolved in a NaOH solution (25mL) with a concentration of 1.44g / mL, stirred for 20h, 2mL of epichlorohydrin was added, and then 0.3g of cuttlefish powder was added. The mixture was frozen for 2h and freeze-dried for 48h to obtain a multifunctional all-biomass aerogel with photothermal conversion capability. Figure 6 and Figure 8 As shown, the aerogel has a self-cleaning function. When 1g of NaCl solid is placed on its surface, it completely disappears within 50 minutes, indicating that it can achieve a self-cleaning function when there is salt contamination on the surface.
Claims
1. A method for preparing a multifunctional all-biomass aerogel with light-to-heat conversion capability, characterized in that: The cellulose nanofibers and hydroxyapatite nanowires were dissolved in an alkaline solution and stirred to form a uniform slurry, and then cuttlefish powder and a cross-linking agent were added and stirred evenly, and then placed in a refrigerator for freezing, and then freeze-dried to obtain a multifunctional all-biomass aerogel with photothermal conversion capability; Among them, the mass ratio of cellulose nanofibers, hydroxyapatite nanowires and cuttlefish powder is (3-4):(1-2):(1-3), and the mass ratio of alkaline solution to cellulose nanofibers is (90-2):
1.
2. The method for preparing a multifunctional all-biomass aerogel with light-to-heat conversion capability according to claim 1, characterized in that: The alkaline solution is sodium hydroxide and / or potassium hydroxide.
3. The method for preparing the multifunctional all-biomass aerogel with light-to-heat conversion capability according to claim 1, characterized in that: The cross-linking agent is epichlorohydrin and / or glutaraldehyde.
4. The method for preparing a multifunctional all-biomass aerogel with light-to-heat conversion capability according to claim 1, characterized in that: The freezing time is 2 to 10 hours, and the freeze-drying time is 24 to 48 hours.
5. The method for preparing a multifunctional all-biomass aerogel with light-to-heat conversion capability according to claim 1, characterized in that: The cellulose nanofiber and hydroxyapatite nanowire solution is stirred for 18 to 24 hours.
6. The method for preparing a multifunctional all-biomass aerogel with light-to-heat conversion capability according to claim 1, characterized in that The cellulose nanofibers are prepared by the following method: The raw material containing cellulose is dried, and lignin is removed and extracted using an inorganic solution in a heated oil bath magnetic stirrer. After drying, the raw material is crushed using a crusher to obtain cellulose nanofibers.
7. The method for preparing a multifunctional all-biomass aerogel with light-to-heat conversion capability according to claim 6, characterized in that: The raw materials containing cellulose are crop straw, flax, cotton, industrial hemp and wood; the raw materials are placed in a vertical blast drying oven, the temperature of the oven is 60-100° C., and the drying time is 24-48 hours.
8. The method for preparing the multifunctional all-biomass aerogel with light-to-heat conversion capability according to claim 6, characterized in that: The inorganic solvent for removing lignin is a mixture of one or more of sodium chlorite, acetic acid and propionic acid; the concentration of the inorganic solution for removing lignin is 0.005-3.0 g / mL, and the mass ratio of the inorganic solution for removing lignin to the dried cellulose-containing raw material is (50-300):1; The solvent for extracting cellulose nanofibers is a mixture of sodium hydroxide, potassium hydroxide or one or more thereof; the concentration of the cellulose nanofiber extraction solution is 0.005-3.0 g / mL, and the mass ratio of the cellulose extraction solution to the extracted cellulose is (50-300):
1.
9. The method for preparing the multifunctional all-biomass aerogel with light-to-heat conversion capability according to claim 6, characterized in that: The heating oil bath magnetic stirrer has a heat preservation temperature of 50 to 200° C. and a heat preservation time of 4 to 20 hours.
10. The method for preparing a multifunctional all-biomass aerogel with light-to-heat conversion capability according to claim 1, characterized in that The hydroxyapatite nanowires are prepared by the following method: 10 mL of 0.05 g / mL sodium hydroxide solution, 10 mL of 0.0176 g / mL calcium chloride solution and 10 mL of 0.023 g / mL anhydrous sodium dihydrogen phosphate solution were added dropwise to 7.128 g of oleic acid and 9 mL of anhydrous ethanol, stirred, and hydrothermally reacted for 12-24 h. The hydroxyapatite nanowires were obtained after reacting in a vertical forced air drying oven at 180° C. for 24 h.
Citation Information
Patent Citations
Flame-retardant microcrystalline cellulose / hydroxyapatite composite aerogel and preparation method thereof
CN108238595A
Cellulose-based photo-thermal conversion gel material and preparation method thereof
CN111040254A
Preparation method of nanocellulose / hydroxyapatite nanospheres
CN111690155A
Nano-hydroxyapatite / silk fibroin / cellulose composite aerogel and preparation method thereof
CN112957525A
Cellulose nanofiber aerogel photo-thermal interface water evaporation material and preparation method thereof
CN114405421A