Bentonite / chitosan / gamma-polyglutamic acid nano material as well as preparation method and application thereof
The bentonite/chitosan/γ-polyglutamic acid nanomaterials prepared by stirring reaction in acetic acid solution solves the problem of insufficient adsorption capacity of existing nanoparticles on heavy metals, and achieves efficient heavy metal adsorption and antibacterial properties, simplifying the The process flow is suitable for practical applications.
Patent Information
- Application Number
- CN202411070978.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-22
AI Technical Summary
The existing environmentally friendly nanoparticles have poor adsorption ability to heavy metal ions, and the traditional nanoparticle synthesis method is complex and cumbersome.
The polymerization reaction is used to combine nanobentonite with chitosan and γ-polyglutamic acid through ionic bonds to prepare bentonite/chitosan/γ-polyglutamic acid nanomaterials with high stability and uniform particles, and then use it to acetic acid solution. The reaction is stirred in the process to control the particle size and Zeta potential, and optimize the preparation conditions of nanoparticles.
The prepared nanomaterials have excellent heavy metal adsorption ability and antibacterial properties, and are suitable for the application of heavy metal adsorption and antibacterial agents. The process is simple and easy to industrialize.
Smart Images

Figure CN118988257A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nanomaterials, and in particular to a bentonite / chitosan / gamma-polyglutamic acid nanomaterial and a preparation method and application thereof. Background Art
[0002] Heavy metal pollution mainly comes from a series of elements with significant biological toxicity, such as mercury, cadmium, lead, chromium and metalloid arsenic, as well as other toxic heavy metals such as zinc, copper, cobalt, nickel, tin, vanadium, etc. At present, the prevention and control of heavy metal pollution has become an important focus in the field of environmental research. Regarding the treatment methods of heavy metals, there are not only conventional chemical precipitation, electrolysis, and membrane separation methods, but also some relatively novel and environmentally friendly unconventional treatment methods that have been developed in recent years, including adsorption, nanotechnology and biological treatment. The main principle of heavy metal treatment is to transform the highly toxic and soluble form into a less toxic, less soluble or insoluble form.
[0003] At present, the use of nanoparticles to treat heavy metal pollution has become a research hotspot. Huang Biao and others used the new environmentally friendly material LDHs to carry out heavy metal contaminated soil passivation remediation experiments in Yongfeng Village, Chengxiang Town, Taicang City and Tianfu Village, Huaqiao Town, Kunshan City. The long-term effects of passivators on soil properties, the stability of heavy metals after passivation, and the most suitable application dosage under different soil characteristics and pollution levels were studied. Experimental data showed that after applying LDHs-01, the Cd content in rice grains was 0.12 and 0.10 mg / kg, respectively. -1 Compared with the control group, this content decreased by 69.2% and 74.4%. Jia Jin et al. used the functional groups of a large number of primary, secondary and tertiary amines in the molecular chain of branched polyethyleneimine to strongly chelate and adsorb heavy metal ions. The results showed that PEI has a strong chelating effect on Cu 2+ The maximum adsorption capacity can reach 227.6 mg / g.
[0004] It is known that nanoparticles can 2+ 、Ni 2+ Cr 3+ , Mn 2+ 、Al 3+ Heavy metal ions such as iodine and iodine have good adsorption capacity, but the traditional synthesis of nanoparticles is not easy to achieve and the process is cumbersome. At present, there is no report on the use of bentonite, chitosan and polyglutamic acid to prepare nanoparticles and conduct in-depth research on their heavy metal adsorption. This technology helps to enrich the theory of nanoparticle preparation and provide strong support for the development of nanoparticle materials for heavy metal adsorption, thereby increasing the application of nanoparticles for heavy metal adsorption in actual processes. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a bentonite / chitosan / γ-polyglutamic acid nanomaterial and a preparation method and application thereof, so as to solve the problem that the existing environmentally friendly nanoparticles have poor adsorption capacity for heavy metal ions.
[0006] To achieve the above purpose and other related purposes, the present invention provides a method for preparing a bentonite / chitosan / γ-polyglutamic acid nanomaterial, wherein nano bentonite is dispersed in an acetic acid solution of chitosan, γ-polyglutamic acid is added, and the mixture is stirred for reaction to obtain the bentonite / chitosan / γ-polyglutamic acid nanomaterial.
[0007] Preferably, the preparation method of the chitosan acetic acid solution is: dissolving chitosan in 5% acetic acid solution.
[0008] Preferably, the mass concentration of chitosan in the chitosan acetic acid solution is 0.5-4 mg / mL.
[0009] Preferably, the amount of the nano-bentonite added to the chitosan acetic acid solution is 0.5-4 mg / mL.
[0010] Preferably, the mass ratio of the γ-polyglutamic acid to chitosan (PGA-CS) is 1:(1-10).
[0011] Preferably, the stirring reaction time is 55 to 65 minutes.
[0012] In the above technical solution of the present application, the dosage of the parameters affects the relationship between particle size and Zeta potential. For example, the PGA-CS mass ratio can determine the size of the particle size, but it will also affect the Zeta potential; while the chitosan mass concentration has a decisive effect on the Zeta potential and can also change the particle size. When the particle size is small, the increase in the chitosan mass concentration will cause the particle size of the bentonite / chitosan / polyglutamic acid nanoparticles to increase, thereby reducing the Zeta potential accordingly. However, too high a concentration is not conducive to the stability of the nanoparticles, but will have an adverse effect on their Zeta potential. Therefore, a smaller particle size and a higher Zeta potential were selected as the best optimization conditions.
[0013] Preferably, the method for preparing the nano bentonite comprises the following steps: (1) wet-milling bentonite and passing it through a 200-mesh sieve to obtain purified bentonite; (2) acidifying the purified bentonite to obtain acidified bentonite; (3) adding the aminosilane coupling agent into an ethanol aqueous solution for hydrolysis to obtain an aminosilane coupling agent hydrolyzate; (4) adding the acidified bentonite to the hydrolysis of the aminosilane coupling agent, stirring the reaction, washing, drying, grinding, and sieving to obtain nano bentonite.
[0014] Preferably, in step (2), the acidification treatment is as follows: adding the purified bentonite to a 15% hydrochloric acid solution, placing the mixture in a water bath at 85-95° C., stirring at a speed of 500-600 r / min for 5-6 hours, wherein the solid-to-liquid ratio of the purified bentonite to the 15% hydrochloric acid solution is 1:(4-5), centrifuging and washing until the pH value of the filtrate is 5-6, drying, cooling to room temperature, grinding and crushing to obtain acidified bentonite.
[0015] Preferably, in step (3), the volume ratio of ethanol to water in the ethanol aqueous solution is (2-3):1, the volume ratio of the aminosilane coupling agent to the ethanol aqueous solution is 1:(9-11), the pH value of the reaction system is controlled to be 3-4 during the hydrolysis process, the hydrolysis temperature is 65-75°C, and the hydrolysis time is 2.5-3.5h; in step (4), the temperature of the stirring reaction is 65-75°C.
[0016] The present invention also provides a bentonite / chitosan / γ-polyglutamic acid nano material prepared by the above preparation method.
[0017] The present invention also provides an application of bentonite / chitosan / γ-polyglutamic acid nanomaterial as an adsorbent in heavy metal adsorption.
[0018] The present invention also provides an application of bentonite / chitosan / γ-polyglutamic acid nanomaterial as an effective component in the preparation of an antibacterial agent.
[0019] As described above, the present invention has the following beneficial effects: (1) The present invention adopts a polymerization reaction to combine nano-bentonite with chitosan and γ-polyglutamic acid in the form of ionic bonds to obtain a bentonite / chitosan / γ-polyglutamic acid nanomaterial with high stability and uniform particles. The experimental steps are simple, the process conditions are easy to control, and it is easy to industrialize; (2) The bentonite / chitosan / γ-polyglutamic acid nanomaterial prepared by the preparation method of the present invention has an adsorption group that can capture the target nuclide and has excellent heavy metal adsorption capacity and antibacterial performance; (3) The bentonite / chitosan / γ-polyglutamic acid nanomaterial prepared by the present invention can be used as an adsorbent in heavy metal adsorption and as an effective ingredient in the preparation of antibacterial agents, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The graphs show the particle size and Zeta potential of bentonite / chitosan / γ-polyglutamic acid nanomaterials prepared at different nano-bentonite mass concentrations in Examples 1 to 5.
[0021] Figure 2The graphs show the particle size and Zeta potential of bentonite / chitosan / γ-polyglutamic acid nanomaterials prepared at different chitosan mass concentrations in Examples 1 and 6-9.
[0022] Figure 3 The graphs show the particle size and Zeta potential of bentonite / chitosan / γ-polyglutamic acid nanomaterials prepared with different mass ratios of γ-polyglutamic acid to chitosan (PGA-CS) in Examples 1 and 10 to 13.
[0023] Figure 4 The graphs show the particle size and Zeta potential of bentonite / chitosan / γ-polyglutamic acid nanomaterials prepared at different stirring times in Example 1 and Comparative Examples 1 to 3.
[0024] Figure 5 Shown are infrared spectra of chitosan (CS), bentonite (MMT), γ-polyglutamic acid (γ-PGA) and bentonite / chitosan / γ-polyglutamic acid nanomaterial (Nanoparticle) prepared in Example 14.
[0025] Figure 6 Shown is a cobalt standard curve.
[0026] Figure 7 Shown is the curve of the cobalt adsorption amount of the bentonite / chitosan / polyglutamic acid nanomaterial prepared in Example 14 changing with time.
[0027] Figure 8 The graph shows the antibacterial effect of the bentonite / chitosan / polyglutamic acid nanomaterial prepared in Example 14 on Escherichia coli: A: cultured at 37°C for one day; B: cultured at 37°C for two days; C: cultured at 37°C for three days; D: cultured at 37°C for four days. DETAILED DESCRIPTION
[0028] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0029] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.
[0030] In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in the present invention does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these explicitly mentioned two devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0031] The reagents required in the preparation process of bentonite / chitosan / polyglutamic acid nanomaterials in the following examples of the present application are as follows: 15% (v / v) hydrochloric acid solution: 15 mL of hydrochloric acid is dissolved in 85 mL of water; ethanol aqueous solution: 75 mL of anhydrous ethanol is dissolved in 25 mL of water; 5% (v / v) acetic acid solution: 5 mL of anhydrous ethanol is dissolved in 95 mL of water; polyglutamic acid aqueous solution: a certain mass of polyglutamic acid is weighed and dissolved in a certain amount of water.
[0032] Example 1 The present application provides a method for preparing a bentonite / chitosan / γ-polyglutamic acid nanomaterial, comprising: (I) Preparation of nano bentonite: (1) Dissolve 10 g of bentonite in 100 ml of water, stir at 300 r / min for 3 h, centrifuge for 10 min (speed is 3000 r / min), dry and grind, and pass through a 200-mesh molecular sieve to obtain purified bentonite; (2) adding the purified bentonite to a 15% hydrochloric acid solution with a solid-liquid ratio of 1 to 5, stirring in a water bath at 90° C. and 500 rpm for 5 h, centrifuging and washing until the pH of the filtrate is 5-6, then drying, naturally cooling to room temperature, grinding and pulverizing to obtain acidified bentonite; (3) adding the aminosilane coupling agent to an ethanol aqueous solution for hydrolysis, wherein the volume ratio of ethanol to water in the ethanol aqueous solution is 3:1, and the volume ratio of the aminosilane coupling agent to the ethanol aqueous solution is 1:10, stirring gently at a speed of 100 rpm, and adding a small amount of 37% hydrochloric acid solution to adjust the pH value of the mixture to 3-4, and maintaining the hydrolysis reaction temperature at 70°C for 3 hours to obtain an aminosilane coupling agent hydrolyzate; (4) Adding the acidified bentonite to the aminosilane coupling agent, the reaction temperature is still maintained at 70°C, and the stirring speed is increased to 200 r / min for stirring for 3 hours; then the mixture is stabilized for 24 hours before filtering, and then washed several times with ethanol water to remove excess aminosilane coupling agent; it is filtered and dried at 80°C, ground and sieved to obtain nano bentonite.
[0033] (II) Preparation of bentonite / chitosan / γ-polyglutamic acid nanomaterials: Dissolve chitosan in a 5% acetic acid solution, and stir at room temperature for 2 hours to make the solution clear and transparent, wherein the mass concentration of chitosan in the chitosan acetic acid solution is 2 mg / mL; Use a pipette to accurately transfer 20 mL of chitosan solution into a beaker, add nano-bentonite, and stir for 1 hour to make the solution clear and transparent; the amount of nano-bentonite added to the chitosan acetic acid solution is 2 mg / mL; 20 mL of γ-polyglutamic acid (PGA) aqueous solution was slowly added dropwise, the mass ratio of γ-polyglutamic acid to chitosan was 1:2 (0.5), and after the addition of the PGA aqueous solution was completed, magnetic stirring was continued for 60 minutes to obtain bentonite / chitosan / polyglutamic acid nanomaterials.
[0034] Embodiments 2 to 5 Examples 2 to 5 of the present application provide a method for preparing a bentonite / chitosan / γ-polyglutamic acid nanomaterial, comprising: (I) Preparation of nano-bentonite: refer to Example 1, which will not be described in detail here; (II) Preparation of bentonite / chitosan / γ-polyglutamic acid nanomaterials: In this step, the difference between Examples 2 to 4 and Example 1 is that the amount of nano-bentonite added to the chitosan acetic acid solution is different, namely 0.5 mg / mL, 1.0 mg / mL, 3.0 mg / mL, and 4.0 mg / mL; The particle size and Zeta potential of bentonite / chitosan / γ-polyglutamic acid nanomaterials prepared by using different nano-bentonite mass concentrations in Examples 1 to 4 are shown in FIG. Figure 1 As shown, from Figure 1It can be seen that when the mass concentration of nano-bentonite in Example 1 is 2 mg / mL, the particle size reaches the minimum, which is about 326.7 nm. Then, as the mass concentration of bentonite continues to increase, the particle size increases rapidly. This may be because there is an excess of bentonite, and the excess bentonite cannot form nanoparticles with chitosan and polyglutamic acid. The bentonite combines with the bentonite to form larger particles, resulting in a rapid increase in particle size. In terms of Zeta, it shows a trend of first increasing and then decreasing. When the mass concentration of bentonite is 2 mg / mL, the Zeta potential is the highest. This is because the prepared bentonite / chitosan / polyglutamic acid nanoparticles have a smaller and more stable particle size, but the overall difference is not large.
[0035] Embodiments 6 to 9 Examples 6 to 9 of the present application provide a method for preparing a bentonite / chitosan / γ-polyglutamic acid nanomaterial, comprising: (I) Preparation of nano-bentonite: refer to Example 1, which will not be described in detail here; (II) Preparation of bentonite / chitosan / γ-polyglutamic acid nanomaterials: In this step, the difference between Examples 6 to 9 and Example 1 is that the mass concentration of chitosan in the chitosan acetic acid solution is different, namely 0.5 mg / mL, 1 mg / mL, 3 mg / mL, and 4 mg / mL; The particle size and Zeta potential of bentonite / chitosan / γ-polyglutamic acid nanomaterials prepared in Examples 1 and 6 to 9 using different chitosan mass concentrations are shown in the figure. Figure 2 As shown, from Figure 2 It can be seen that: as the chitosan mass concentration increases, the particle size gradually increases. When the chitosan mass concentration is between 2 mg / mL and 3 mg / mL, the nanoparticle size increases the most, increasing by about 387 nm. This may be because the chitosan is excessive, and the free chitosan forms larger particles with polyglutamic acid, resulting in a rapid increase in the particle size. In terms of Zeta, it shows a trend of first increasing and then decreasing. In Example 1, when the chitosan mass concentration is 2 mg / mL, the Zeta potential is the highest. This may be because when the chitosan concentration is low, not only bentonite / chitosan / polyglutamic acid nanoparticles are formed, but also a certain amount of bentonite / polyglutamic acid nanoparticles exist, and the bentonite / polyglutamic acid nanoparticles have a low Zeta potential. As the chitosan mass concentration increases, it is more conducive to the formation of bentonite / chitosan / polyglutamic acid nanoparticles, and the Zeta potential increases. When the chitosan is excessive, the free chitosan will reduce the stability of the prepared sample.
[0036] Embodiments 10 to 13 Examples 11 to 13 of the present application provide a method for preparing a bentonite / chitosan / γ-polyglutamic acid nanomaterial, comprising: (I) Preparation of nano-bentonite: refer to Example 1, which will not be described in detail here; (II) Preparation of bentonite / chitosan / γ-polyglutamic acid nanomaterials: In this step, Examples 10 to 13 differ from Example 1 in that the mass ratios of γ-polyglutamic acid to chitosan are different, namely 1:10 (0.1), 1:4 (0.25), 3:4 (0.75) and 1:1 (1), respectively.
[0037] The particle size and Zeta potential of bentonite / chitosan / γ-polyglutamic acid nanomaterials prepared by different mass ratios of γ-polyglutamic acid to chitosan (PGA-CS) in Examples 1 and 10 to 13 are shown in FIG. Figure 3 As shown, from Figure 3 It can be seen that as the PGA-CS mass ratio increases, the particle size first decreases and then gradually increases, especially when the PGA-CS mass ratio in Example 1 is 1:2, the nanoparticle size is the smallest, which is about 326.7 nm. This is because when the polyglutamic acid is less, bentonite and bentonite, bentonite and chitosan combine into larger particles, resulting in a large particle size. As the polyglutamic acid content increases, the presence of bentonite / chitosan / polyglutamic acid nanoparticles reduces the average particle size, and the Zeta shows a decrease first, then an increase, and then a decrease. This shows that when polyglutamic acid is insufficient or excessive, it is not conducive to the stability of the prepared nanoparticles.
[0038] Comparative Examples 1 to 3 Comparative Examples 1 to 3 of the present application provide a method for preparing a bentonite / chitosan / γ-polyglutamic acid nanomaterial, comprising: (I) Preparation of nano-bentonite: refer to Example 1, which will not be described in detail here; (II) Preparation of bentonite / chitosan / γ-polyglutamic acid nanomaterials: In this step, the difference between Comparative Examples 1 to 3 and Example 1 is that the stirring time is different, namely 0 min, 30 min and 90 min, respectively.
[0039] The particle size and Zeta potential of bentonite / chitosan / γ-polyglutamic acid nanomaterials prepared at different stirring times in Example 1 and Comparative Examples 1 to 3 are shown in FIG. Figure 4 As shown, from Figure 4It can be seen that the formation of bentonite / chitosan / polyglutamic acid nanoparticles requires appropriate stirring time, and when embodiment 1 adopts stirring time for 60min, the prepared nanoparticle stability is the best, and particle diameter can reach 326.7nm, and Zeta potential is about 53.4mV. Because the formation of bentonite / chitosan / polyglutamic acid nanoparticles is a dynamic process, when stirring time is suitable, it is conducive to the formation of uniform nanoparticles and the dispersion of each material, and when stirring time is too long, the interaction between nanoparticles will be destroyed, thereby causing bentonite / chitosan / polyglutamic acid nanoparticle structure to be destroyed and affect its stability. From the results of 4 single factors, stirring time, bentonite mass concentration, chitosan mass concentration and PGA-CS mass ratio have a significant impact on nanoparticle formation, and the nanoparticles formed by stirring time 60min are shown to be better by the early experimental phenomenon, and therefore, the most preferred stirring time is 60min.
[0040] Embodiment 14 The present application provides a method for preparing a bentonite / chitosan / γ-polyglutamic acid nanomaterial, comprising: (I) Preparation of nano-bentonite: refer to Example 1, which will not be described in detail here; (II) Preparation of bentonite / chitosan / γ-polyglutamic acid nanomaterials: Dissolve chitosan in a 5% acetic acid solution, and stir at room temperature for 2 hours to make the solution clear and transparent, wherein the mass concentration of chitosan in the chitosan acetic acid solution is 2.0 mg / mL; Use a pipette to accurately transfer 20 mL of chitosan solution into a beaker, add nano-bentonite, and stir for 1 hour to make the solution clear and transparent; the amount of nano-bentonite added to the chitosan acetic acid solution is 2.18 mg / mL; 20 mL of γ-polyglutamic acid (PGA) aqueous solution was slowly added dropwise, the mass ratio of γ-polyglutamic acid to chitosan was 1:4 (0.25), and after the addition of the PGA aqueous solution was completed, magnetic stirring was continued for 60 minutes to obtain bentonite / chitosan / polyglutamic acid nanomaterials.
[0041] The average particle size of the bentonite / chitosan / polyglutamic acid nanomaterial prepared in this example is 899.76 nm, and the Zeta potential is 60.57 mV.
[0042] The infrared spectra of chitosan (CS), bentonite (MMT), γ-polyglutamic acid (γ-PGA) and bentonite / chitosan / polyglutamic acid nanoparticles prepared in Example 14 were collected using a Fourier transform infrared spectrometer KBr tablet method. The collection conditions were: temperature at 25°C, resolution of 4 cm -1 , 500~4000cm -1The wave number range was scanned 32 times, and the obtained infrared data were imported into the origin software for plotting and analysis. The results are as follows Figure 5 as shown. from Figure 5 It can be seen that: in the chitosan CS spectrum, 1071 cm -1 The COC skeleton vibration peak at 3523 cm-1 no longer exists in the nanoparticle spectrum, indicating that the CS polysaccharide chain has been reorganized and its skeleton structure has been rearranged inside the nanoparticle. At the same time, the stretching vibration characteristic peaks of the hydroxyl and amino functional groups at 3523 cm-1 -1 and 3607cm -1 The functional groups are retained, indicating that they are still present in the synthesized nanoparticles. -1 The strong peak at 1641 cm is attributed to the stretching vibration peak of Al-OH-Al. -1 The absorption peak at 1035cm is the bending vibration peak of adsorbed water and zeolite water in the channel. -1 The peak at 789cm is the stretching vibration peak of the silicon-oxygen bond. -1 The peak at 1045cm is the vibration peak of silica quartz impurities. -1 The Si-O vibration characteristic peak at 1478 cm-1 disappeared in the nanoparticle spectrum, confirming that the interlayer silicon-oxygen structure of MMT was adjusted during the synthesis process. -1 Move to 1663cm -1 , reflecting the change in electron density of the carboxyl environment.
[0043] 534cm -1 and 670cm -1 The peak at 1537cm may be related to the metal oxide vibration of the MMT mineral component, indicating the interaction between the inorganic-organic components. -1 and 1428cm -1 The peak at 1655cm matches the amide II band, which directly indicates that the amide groups of CS interact with the carboxyl functional groups of γ-PGA, which may be achieved through hydrogen bonding or covalent bonding. -1 The amide groups at the chitosan site (some amide groups are still present in chitosan) may be slightly red-shifted to 1647 cm after polymerization to form nanoparticles. -1 The protonated chitosan may be ammonium cationic salt (-NH 3+ ) in the form of ionic bonding with bentonite. 3338cm -1 、3459cm -1 、3543cm -1 and 3603cm -1The peaks at 400 nm intensify the stretching vibrations of OH and NH, and the retention of these peaks emphasizes the central role of hydrogen bonding in the stability of the nanoparticles.
[0044] In general, in the whole polymerization reaction, bentonite combines with chitosan and polyglutamic acid in the form of ionic bonds, and the primary amine group peak of chitosan decreases or disappears after polymerization, indicating that it may combine with the carboxyl group of polyglutamic acid, while the -OH and NH as adsorption groups are still intact, indicating that bentonite, chitosan and polyglutamic acid are well combined, and there are still adsorption groups that can capture the target nuclides.
[0045] The present application also provides an application of bentonite / chitosan / polyglutamic acid nanomaterial prepared in Example 14 as an adsorbent in heavy metal adsorption, comprising the following steps: (1) Sample pretreatment 20 mL of a cobalt nitrate solution having a molar concentration of 0.16 mol / L was mixed with 20 mL of the bentonite / chitosan / polyglutamic acid nanoparticle adsorbent prepared in Example 14, and an adsorption experiment was performed under magnetic stirring for a certain period of time at normal temperature and pressure (speed of 200 r / min), and the supernatant was filtered with a 0.22 μm filter membrane, and the sample pretreatment was completed.
[0046] (2) Drawing of standard curve The prepared Co with concentrations of 0.04, 0.06, 0.08, 0.1, 0.12, 0.14, and 0.16 mol / L was measured at a wavelength of λmax=512 nm. 2+ The solution was tested for absorbance, and the experimental data were linearly fitted to obtain a linear relationship.
[0047] Co 2+ The solution concentration (mol / L) is used as the horizontal axis and the absorbance (A) is used as the vertical axis to draw the standard curve. Figure 6 It can be seen from the figure that the linear range of this method is 0-0.16 mol / L, the regression equation is y=4.7708x-0.00007, and the correlation coefficient r=0.9994.
[0048] (3) Determination of cobalt content in samples Pipette 5.00mL of sample and perform the above operations according to the standard curve experiment. Calculate using formula 2.2: Wherein: A = absorbance value of sample measurement; A0 = absorbance value of reagent blank measurement; a = regression equation intercept; b = regression equation slope; V = sample volume (mL).
[0049] (4) Calculation of heavy metal adsorption formula The supernatant liquid of the sample was taken and the content of Co(II) in the solution after nanoparticle adsorption was determined by an ultraviolet spectrophotometer. The adsorption performance of the nanoparticles on Co(II) was evaluated by the adsorption amount Q shown in formula 2.3.
[0050] Where: Q = adsorption amount of heavy metals by nanoparticles (mmol / g); C0 = initial concentration of heavy metals in solution (mol / L); C t = concentration when adsorption equilibrium is reached (mol / L); V = volume of adsorption system (mL); m = mass of adsorbent (g).
[0051] Curve of cobalt adsorption changing with time Figure 7 As shown, from Figure 7 It can be seen that the adsorption amount of cobalt increases with time, but its growth rate decreases with time. The initial concentration of heavy metals in the solution before adsorption is 80mmol / L, and the concentration C0 when adsorption equilibrium is reached at 135min is t The adsorption capacity Q is 59.6mmol / L, and the adsorption capacity Q is 17.4mmol / g. Although bentonite, chitosan and γ-polyglutamic acid each have a certain adsorption capacity, when they are composited to form nanoparticles, their internal active sites may be restricted, resulting in a decrease in the adsorption capacity for cobalt ions. In addition, the surface area and pore structure of nanoparticles are also key factors affecting the adsorption performance. And because the surface area of nanoparticles is small or the pore structure is not well developed, their adsorption capacity for cobalt ions will naturally be affected.
[0052] The present application also provides an antibacterial test of the bentonite / chitosan / polyglutamic acid nanomaterial prepared in Example 14. Antibacterial test refers to the in vitro determination of the antibacterial or bactericidal ability of a sample. When the growth of bacteria is inhibited, a transparent antibacterial circle will appear. By measuring the size of the antibacterial circle, the degree of inhibition of a certain substance on the indicator bacteria is judged. Generally speaking, the larger the diameter of the antibacterial circle, the better the antibacterial effect of the substance on a certain bacteria. Escherichia coli is a bacterium existing in the intestines of humans and many animals, and its types and numbers are quite large. This test selects Escherichia coli as an intestinal indicator bacteria, and the degree of inhibition of bentonite / chitosan / polyglutamic acid nanoparticles on Escherichia coli is tested by measuring the size of the antibacterial circle.
[0053] (1) Preparation of culture medium: Add 10g of nutrient agar medium into a beaker, add 1000mL of distilled water, and after it is completely dissolved, divide it into Erlenmeyer flasks and plug them with cotton plugs. Sterilize the above medium in a 0.1Mpa, 121℃ high pressure sterilizer for 30min. After sterilization, prepare the plate immediately and cool it to about 45℃ for use.
[0054] (2) Inoculation of Escherichia coli: In the clean bench, the E. coli stored in the refrigerator was inoculated onto the plate culture medium by streak inoculation method. After culturing in a 37°C constant temperature incubator for 24 hours, a single colony with good growth was picked with an inoculation loop to prepare 10 6 cfu / mL concentration of Escherichia coli suspension, and aspirate 0.1mL of the bacterial suspension onto the plate culture medium, spread it evenly with a sterile applicator, and place it flat for 20 minutes to allow the bacteria to fully penetrate into the culture medium, and then use tweezers to place the sterilized Oxford cup into the above-mentioned culture dish.
[0055] (3) Determination of inhibition zone: 200 μL of the bentonite / chitosan / polyglutamic acid nanomaterials prepared in Example 14 were respectively injected into three Oxford cups. After the bentonite / chitosan / polyglutamic acid nanoparticles were fully mixed with the culture medium, the Oxford cups were taken out, sealed with sealing film, and placed in a constant temperature incubator at 37°C for 4 days. The sizes of the inhibition zones were observed, photographed, and recorded. The results are as follows: Figure 8 shown.
[0056] from Figure 8 It can be seen that the colonies of Escherichia coli are round, milky white, with neat edges, smooth surfaces, and basically the same color. The size of the inhibition zone reflects the degree of inhibition of the indicator bacteria by the drug. Combined with the figure, it can be seen that the bentonite / chitosan / polyglutamic acid nanoparticles do not have obvious antibacterial properties in general. The diameter of the inhibition zone increased from 0 mm to 2 mm on the first and second days, showing a very weak antibacterial phenomenon. The inhibition zone gradually disappeared from the second day and completely disappeared on the fourth day. This shows that the bentonite / chitosan / polyglutamic acid nanomaterials prepared in this application have certain antibacterial properties.
[0057] In summary, the present invention adopts polymerization reaction to combine nano bentonite with chitosan and γ-polyglutamic acid in the form of ionic bonds to obtain bentonite / chitosan / γ-polyglutamic acid nanomaterials with high stability and uniform particles, and the experimental steps are simple, the process conditions are easy to control, and it is easy to industrialize; the bentonite / chitosan / γ-polyglutamic acid nanomaterials prepared by the preparation method of the present invention have adsorption groups that can capture target nuclides, and have excellent heavy metal adsorption capacity and antibacterial properties; the bentonite / chitosan / γ-polyglutamic acid nanomaterials prepared by the present invention can be used as an adsorbent in heavy metal adsorption, and as an effective ingredient for preparing antibacterial agents, and have broad application prospects. Therefore, the present invention effectively overcomes the various shortcomings in the prior art and has a high industrial utilization value.
[0058] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for preparing bentonite / chitosan / γ-polyglutamic acid nanomaterial, characterized in that: The nano bentonite is dispersed in the acetic acid solution of chitosan, and gamma-polyglutamic acid is added, and the mixture is stirred for reaction to prepare the bentonite / chitosan / gamma-polyglutamic acid nano material.
2. The preparation method according to claim 1, characterized in that: The preparation method of the chitosan acetic acid solution is as follows: dissolving chitosan in a 5% acetic acid solution; the mass concentration of chitosan in the chitosan acetic acid solution is 0.5-4 mg / mL; and the amount of the nano-bentonite added to the chitosan acetic acid solution is 0.5-4 mg / mL.
3. The preparation method according to claim 1, characterized in that: The mass ratio of the gamma-polyglutamic acid to chitosan is 1:(1-10).
4. The preparation method according to claim 1, characterized in that: The stirring reaction time is 55 to 65 minutes.
5. The preparation method according to claim 1, characterized in that: The preparation method of the nano bentonite comprises the following steps: (1) wet-milling bentonite and passing it through a 200-mesh sieve to obtain purified bentonite; (2) acidifying the purified bentonite to obtain acidified bentonite; (3) adding the aminosilane coupling agent into an ethanol aqueous solution for hydrolysis to obtain an aminosilane coupling agent hydrolyzate; (4) adding the acidified bentonite to the hydrolysis of the aminosilane coupling agent, stirring the reaction, washing, drying, grinding, and sieving to obtain nano bentonite.
6. The preparation method according to claim 5, characterized in that: In step (2), the acidification treatment is as follows: adding the purified bentonite to a 15% hydrochloric acid solution, placing the mixture in a water bath at 85-95° C., stirring at a speed of 500-600 r / min for 5-6 hours, wherein the solid-to-liquid ratio of the purified bentonite to the 15% hydrochloric acid solution is 1:(4-5), centrifuging and washing until the pH value of the filtrate is 5-6, drying, cooling to room temperature, grinding and pulverizing to obtain acidified bentonite.
7. The preparation method according to claim 5, characterized in that: In step (3), the volume ratio of ethanol to water in the ethanol aqueous solution is (2-3):1, the volume ratio of the aminosilane coupling agent to the ethanol aqueous solution is 1:(9-11), the pH value of the reaction system is controlled to be 3-4 during the hydrolysis process, the hydrolysis temperature is 65-75° C., and the hydrolysis time is 2.5-3.5 h; in step (4), the temperature of the stirring reaction is 65-75° C.
8. A bentonite / chitosan / γ-polyglutamic acid nanomaterial prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the bentonite / chitosan / γ-polyglutamic acid nanomaterial as claimed in claim 8 as an adsorbent in heavy metal adsorption.
10. Use of the bentonite / chitosan / γ-polyglutamic acid nanomaterial as claimed in claim 8 as an effective ingredient in the preparation of an antibacterial agent.
Citation Information
Cited By
Antibacterial packaging material and preparation method thereof
CN119350681A