Dechlorination catalyst and preparation method of carbon-based material loaded noble metal palladium catalyst
By using a palladium catalyst prepared by mixing modified activated carbon with a carbon-based material support and a dimethylaminoethanol palladium nitrate solution, the palladium carbon catalyst in the prior art is solved, and the palladium carbon catalyst is insufficient in the dechlorination reaction, thereby achieving the problem of instability in the prior art. It has high reactivity and stability, and has good anti-toxicity and multiple application capabilities.
Patent Information
- Application Number
- CN202411081369.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-08
AI Technical Summary
The existing palladium carbon catalysts have problems of unstable activity and insufficient selectivity in the dechlorination reaction, and it is difficult to take into account both high reaction activity and stability.
The noble metal palladium catalyst is prepared by using mixed modified activated carbon and carbon-based materials as support, and palladium nitrate solution containing dimethylaminoethanol for adsorption and reduction. By controlling the type and amount of metal, a carbon-based material support with core-shell structure is formed to increase the catalyst. reactivity and stability.
The high reactivity and stability of the palladium catalyst in the dechlorination reaction is achieved, the uncontrollable and loss of metal dosage is avoided, and the anti-toxicity and strong acid-base properties of the catalyst are improved. It can be applied multiple times and the product is highly purified.
Smart Images

Figure CN118988295A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalytic technology, and specifically relates to a preparation method of a dechlorination catalyst and a carbon-based material-loaded noble metal palladium catalyst. Background Art
[0002] 5-Pyrimidinecarboxaldehyde is a commonly used basic raw material for organic synthesis and an intermediate for the synthesis of drug molecules. It has a wide range of applications in organic synthesis. This substance is often used to synthesize other pyrimidine derivatives. Pyrimidine is an important aromatic compound that is widely present in organisms, especially in the structure of nucleic acids (such as DNA and RNA). Pyrimidine and its derivatives play a key role in biology and are an important component of building genetic information and regulating biological processes. 5-Pyrimidinecarboxaldehyde, as a derivative of pyrimidine, can be used to synthesize more complex pyrimidine compounds. 2,3-Dichloropyridine is an important chemical intermediate that is widely used in the fields of pesticides and medicine. It is an important substance for the synthesis of the new insecticide Kangkuan (20% chlorfenapyr). At present, the synthesis of 5-pyrimidinecarboxaldehyde and 2,3-dichloropyridine usually uses palladium-carbon catalyst to catalyze the dechlorination reaction of organic matter 4,6-dichloro-5-pyrimidinecarboxaldehyde and 2,3,4,5-tetrachloropyridine (or 2,3,6-trichloropyridine).
[0003] Palladium-carbon catalysts have the characteristics of small feed amount, high activity, stable performance, green environmental protection and easy recycling. They are widely used in the pharmaceutical industry, petrochemical industry, dye and fragrance industry, electronics industry and other fine chemical reaction processes. When there are one or more side reactions in the product of the catalytic reaction, it is often necessary to balance the relationship between selectivity, activity and catalyst stability. It is particularly important to choose a suitable and efficient catalyst.
[0004] Organic hydrogenation reactions have complex raw materials and reaction processes, and there are many types of palladium-carbon catalysts. In addition, the dechlorination reaction has high requirements for the performance of the catalyst, which requires the catalyst to have stable reaction activity, good selectivity and stability. Therefore, it is particularly important to design and prepare a catalyst that has high activity, selectivity and stability for dechlorination reactions. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a dechlorination catalyst and a preparation method of a carbon-based material-supported noble metal palladium catalyst in view of the above-mentioned deficiencies in the prior art. The preparation method of the present invention comprises using mixed modified activated carbon and carbon-based materials as carriers, using a palladium nitrate solution containing dimethylaminoethanol as a palladium source solution, and preparing a palladium catalyst through adsorption reduction, and the catalyst has high reactivity and stability in the dechlorination reaction.
[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0007] A method for preparing a carbon-based material-supported noble metal palladium catalyst, characterized by comprising:
[0008] Step 1: providing a carbon-based material carrier, specifically comprising:
[0009] Step 101, mixing a salt solution, an organic ligand and an alcohol in a mass ratio of (2-15):(10-50):(35-88), stirring and reacting at 60-100° C. for 8-15 hours to obtain a sol;
[0010] Step 102, drying the sol at 90-150° C. to obtain a gel, crushing the obtained gel and passing it through a 300-500 mesh sieve, and calcining the sieved material at 600-900° C. for 6-12 hours under a N2 atmosphere to obtain a carbon-based material precursor A;
[0011] Step 103, mixing the activated carbon and the carbon-based material precursor A in a mass ratio of (1-9):(9-1), cooking in a nitric acid solution at 90° C. to 100° C. for 1 h to 2 h, cooling, filtering, and washing to obtain an acid-treated carrier;
[0012] Step 104, placing the acid-treated carrier in an ethanol solution of triethylamine, cooking at 90° C. to 100° C. for 1 h to 2 h, cooling and filtering to complete the modification and obtain a carbon-based material carrier;
[0013] Step 2: according to the preset palladium mass percentage in the Pd / C catalyst, the carbon-based material carrier described in step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol, stirred at room temperature for 1 to 3 hours for adsorption, and filtered to obtain a catalyst precursor;
[0014] Step 3: placing the catalyst precursor in a reducing agent solution and stirring for reduction to obtain a carbon-based material-loaded noble metal palladium catalyst.
[0015] The method for preparing the carbon-based material-loaded noble metal palladium catalyst is characterized in that the carbon-based material-loaded noble metal palladium catalyst is a Pd / C catalyst with a Pd mass percentage of 1% to 5%.
[0016] The above-mentioned method for preparing the carbon-based material loaded with precious metal palladium catalyst is characterized in that, in step 101, the salt solution is a metal-soluble salt solution, the organic ligand is one or more of dicyandiamide, thiourea, pyridazine, melamine, cyanuric acid and urea, and the alcohol is methanol or anhydrous ethanol.
[0017] The above-mentioned method for preparing the carbon-based material loaded noble metal palladium catalyst is characterized in that the metal soluble salt is one or more of ferric nitrate, copper nitrate and nickel nitrate.
[0018] The above-mentioned method for preparing the carbon-based material loaded with precious metal palladium catalyst is characterized in that, in step 103, the mass percentage concentration of the nitric acid solution is 5% to 10%, and the mass of the nitric acid solution is 8 to 10 times the total mass of the activated carbon and the carbon-based material precursor A.
[0019] The above-mentioned method for preparing a carbon-based material-supported noble metal palladium catalyst is characterized in that, in step 104, the mass percentage concentration of the ethanol solution of triethylamine is 3%, and the mass of the ethanol solution of triethylamine is 8 to 10 times the mass of the acid-treated carrier.
[0020] The above-mentioned method for preparing the carbon-based material loaded with precious metal palladium catalyst is characterized in that, in step 2, the palladium nitrate solution containing dimethylaminoethanol has a palladium nitrate concentration of 0.1g / ml to 0.5g / ml, and a mass percentage concentration of dimethylaminoethanol is 0.1% to 0.3%.
[0021] The above-mentioned method for preparing a carbon-based material loaded with precious metal palladium catalyst is characterized in that, in step three, the reducing agent solution is a sodium formate solution or a sodium borohydride solution, the mass percentage concentration is 10% to 20%, the stirring reduction temperature is 80°C to 90°C, the stirring reduction time is 1h to 2h, and the mass of the reducing agent solution is 8 to 10 times the mass of the catalyst precursor.
[0022] The above-mentioned method for preparing the carbon-based material loaded with precious metal palladium catalyst is characterized in that, in step 2, it also includes controlling the pH of the system to 8.5 during the adsorption process.
[0023] In addition, the present invention also provides a dechlorination catalyst, characterized in that the dechlorination catalyst is prepared by the above-mentioned preparation method of the carbon-based material loaded noble metal palladium catalyst.
[0024] The reaction equation for the catalytic synthesis of 5-pyrimidinecarboxaldehyde is as follows:
[0025]
[0026] The reaction equation for the catalytic synthesis of 2,3-dichloropyridine is as follows:
[0027]
[0028] The reaction equation for catalytic synthesis of biotin is as follows:
[0029]
[0030] Compared with the prior art, the present invention has the following advantages:
[0031] 1. The present invention provides a method for preparing a carbon-based material-supported noble metal palladium catalyst, the method comprising using mixed modified activated carbon and carbon-based material as carriers, using a palladium nitrate solution containing dimethylaminoethanol as a palladium source solution, and preparing a palladium catalyst by adsorption reduction. The catalyst has high reactivity and stability in a dechlorination reaction.
[0032] 2. The method for preparing a precious metal palladium catalyst loaded on a carbon-based material of the present invention includes preparing a carrier obtained by mixing and modifying activated carbon and a carbon-based material. The carrier is based on a metal salt solution, and the directional adjustment of the carbon-based material and the carrier performance can be achieved by controlling the type and amount of the metal. By mixing the activated carbon with the carbon-based material, the uncontrollable metal dosage and metal loss caused by the metal modification process of the activated carbon can be effectively avoided, and the advantages of the activated carbon and the carbon-based material can be fully combined.
[0033] 3. The preparation method of the carbon-based material loaded with precious metal palladium catalyst of the present invention includes taking metal soluble salt, organic ligand and alcohol as main raw materials, preparing carbon-based material carrier through sol-gel, acid treatment and organic amine modification, taking metal ions in metal soluble salt as core, and forming carbon-based material carrier with core-shell structure after coating with organic ligand, giving the carrier higher physical properties, more uniform component distribution, and richer pore structure, so as to realize synergistic reaction of active components and improve the reaction activity and stability of the catalyst.
[0034] 4. The preparation method of the carbon-based material loaded with precious metal palladium catalyst of the present invention comprises the step of steaming the activated carbon and the carbon-based material precursor with nitric acid, which can give the carrier a developed pore structure and enrich the oxygen-containing functional groups on the surface of the carrier on the basis of fully removing the excess metal ions of the material, so that more metal sites are exposed on the surface of the carrier, so that it can not only combine with the active component Pd, but also promote the adsorption of the easily poisoned catalyst component in the dechlorination reaction, thereby avoiding catalyst poisoning.
[0035] 5. The preparation method of the carbon-based material loaded with precious metal palladium catalyst of the present invention includes using an alcohol solution of triethylamine to modify the acid-treated carrier, which can effectively enrich the groups on the surface of the carrier and regulate the acid and base positions on the surface of the carrier, increase the number of N species on the surface, and improve the catalyst's resistance to poisoning and strong acid and alkali resistance.
[0036] 6. The method for preparing a carbon-based material-loaded noble metal palladium catalyst of the present invention includes using a palladium nitrate solution containing dimethylaminoethanol as a palladium source, which can fully utilize the function of dimethylaminoethanol as a small molecule surfactant to regulate the dispersion speed and dispersion state of Pd on the carrier surface, thereby promoting its stable and uniform distribution on the carrier surface.
[0037] 7. The noble metal palladium supported catalyst prepared by the method of the present invention has a carrier particle size of about 400 meshes, has the advantage of easy solid-liquid separation after the reaction, and can be used multiple times without treating the catalyst after use.
[0038] 8. The dechlorination catalyst of the present invention comprises a mixed modified activated carbon and a carbon-based material as a carrier, a palladium nitrate solution containing dimethylaminoethanol as a palladium source solution, and is prepared by adsorption reduction. The catalyst has high reactivity and stability in the dechlorination reaction.
[0039] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a transmission electron microscope image of the carbon-based material carrier of Example 2. DETAILED DESCRIPTION
[0041] Example 1
[0042] This embodiment provides a method for preparing a carbon-based material-supported noble metal palladium catalyst, wherein the carbon-based material-supported noble metal palladium catalyst is a Pd / C catalyst having a Pd mass percentage of 5%. The preparation method comprises:
[0043] Step 1: providing a carbon-based material carrier, specifically comprising:
[0044] Step 101, mixing a salt solution, an organic ligand and an alcohol in a mass ratio of 10:30:60, stirring and reacting at 80° C. for 10 hours to obtain a sol; the salt solution is a copper nitrate solution with a mass percentage concentration of 0.5 g / ml, the organic ligand is dicyandiamide, and the alcohol is anhydrous ethanol;
[0045] Step 102, drying the sol at 90°C to obtain a gel, crushing the obtained gel and passing it through a 300-mesh sieve, and calcining the sieved material at 600°C for 12h under a N2 atmosphere to obtain a carbon-based material precursor A;
[0046] Step 103, mixing the activated carbon and the carbon-based material precursor A in a mass ratio of 7:3, boiling in a nitric acid solution at 90° C. for 1 hour, cooling and filtering, and washing with pure water until the pH is 5 to obtain an acid-treated carrier; the mass percentage concentration of the nitric acid solution is 5%, and the mass of the nitric acid solution is 10 times the total mass of the activated carbon and the carbon-based material precursor A;
[0047] Step 104, placing the acid-treated carrier in an ethanol solution of 3% triethylamine by mass, boiling at 100° C. for 2 hours, cooling and filtering, completing the modification, and obtaining a carbon-based material carrier; the mass of the ethanol solution of triethylamine is 10 times the mass of the carrier after the acid treatment; the ethanol solution of triethylamine is the ethanol solution of triethylamine obtained by dissolving triethylamine in anhydrous ethanol;
[0048] Step 2: according to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material carrier described in step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol, and stirred at room temperature for 2h for adsorption. During the stirring process, the pH is controlled to 8.5 with a NaOH solution. After the adsorption is completed, the catalyst precursor is obtained by filtering; the palladium nitrate solution containing dimethylaminoethanol is a palladium nitrate solution containing dimethylaminoethanol obtained by dissolving dimethylaminoethanol in a palladium nitrate aqueous solution, the palladium nitrate concentration is 0.5g / ml, the mass percentage concentration of dimethylaminoethanol is 0.3%, and the mass percentage concentration of the above-mentioned NaOH solution is 5%;
[0049] Step three, placing the catalyst precursor in a reducing agent solution and stirring for reduction to obtain a carbon-based material loaded with precious metal palladium catalyst; the reducing agent solution is a sodium borohydride solution with a mass percentage concentration of 20%, the stirring reduction temperature is 80°C, and the stirring reduction time is 2h; the mass of the reducing agent solution is 8 times the mass of the catalyst precursor.
[0050] Example 2
[0051] This embodiment provides a method for preparing a carbon-based material-supported noble metal palladium catalyst, wherein the carbon-based material-supported noble metal palladium catalyst is a Pd / C catalyst having a Pd mass percentage of 3%. The preparation method comprises:
[0052] Step 1: providing a carbon-based material carrier, specifically comprising:
[0053] Step 101, mixing a salt solution, an organic ligand and an alcohol in a mass ratio of 15:50:35, stirring and reacting at 100° C. for 8 hours to obtain a sol; the salt solution is a 0.5 g / ml iron nitrate solution, the organic ligand is thiourea, and the alcohol is methanol;
[0054] Step 102, drying the sol at 150°C to obtain a gel, crushing the obtained gel and passing it through a 350-mesh sieve, and calcining the sieved material at 800°C for 8h under a N2 atmosphere to obtain a carbon-based material precursor A;
[0055] Step 103, mixing the activated carbon and the carbon-based material precursor A in a mass ratio of 7:3, boiling in a nitric acid solution at 90° C. for 2 h, cooling and filtering, and washing with pure water until the pH is 5 to obtain an acid-treated carrier; the mass percentage concentration of the nitric acid solution is 5%, and the mass of the nitric acid solution is 10 times the total mass of the activated carbon and the carbon-based material precursor A;
[0056] Step 104, placing the acid-treated carrier in an ethanol solution with a mass percentage concentration of 3% triethylamine, boiling at 90° C. for 2 hours, cooling and filtering, completing the modification, and obtaining a carbon-based material carrier; the mass of the ethanol solution of triethylamine is 8 times the mass of the carrier after acid treatment;
[0057] Step 2: according to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material carrier described in step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol, and stirred at room temperature for 2h for adsorption. During the stirring process, the pH is controlled to 8.5 with a NaOH solution. After the adsorption is completed, the catalyst precursor is obtained by filtering; in the palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.2g / ml, the mass percentage concentration of dimethylaminoethanol is 0.2%, and the mass percentage concentration of the NaOH solution is 5%;
[0058] Step three, placing the catalyst precursor in a reducing agent solution and stirring for reduction to obtain a carbon-based material loaded with precious metal palladium catalyst; the reducing agent solution is a sodium formate solution with a mass percentage concentration of 20%, the stirring reduction temperature is 90°C, and the stirring reduction time is 1 hour; the mass of the reducing agent solution is 8 times the mass of the catalyst precursor.
[0059] The transmission electron microscope image of the carbon-based material obtained in step 1 of this embodiment is as follows Figure 1 The evaluation results of the structural characteristics of the material are shown in Table 1.
[0060] Table 1 Evaluation results of structural characteristics of carbon-based materials
[0061]
[0062] The evaluation method includes: Experiment 1 is to immerse 100g of the carbon-based material of Example 2 in a hydrochloric acid solution, stir at high speed for 12h, filter to obtain a filtrate, and detect the metal ions in the filtrate by ICP. Experiment 2 is to roast 100g of the carbon-based material of Example 2 at 800°C in an oxygen atmosphere for 6h, dissolve the obtained ash using the above hydrochloric acid solution, filter to obtain a filtrate, and detect the metal ions in the filtrate by ICP.
[0063] According to Table 1, the metal content dissolved by calcining the carbon-based material is much higher than that dissolved by strong acid and mechanical stirring. Due to the organic ligand shell structure of the carbon-based material, the metal inside will not seep into the filtrate. Figure 1 As can be seen from Table 1, the carbon-based material of the present invention is a core-shell structure with higher physical properties.
[0064] Example 3
[0065] This embodiment provides a method for preparing a carbon-based material-supported noble metal palladium catalyst, wherein the carbon-based material-supported noble metal palladium catalyst is a Pd / C catalyst having a Pd mass percentage of 2%, and the preparation method comprises:
[0066] Step 1: providing a carbon-based material carrier, specifically comprising:
[0067] Step 101, mixing a salt solution, an organic ligand and an alcohol in a mass ratio of 5:40:55, stirring and reacting at 90° C. for 15 hours to obtain a sol; the salt solution is a 0.5 g / ml iron nitrate solution, the organic ligand is pyridazine, and the alcohol is methanol;
[0068] Step 102, drying the sol at 130° C. to obtain a gel, crushing the obtained gel and passing it through a 400-mesh sieve, and calcining the sieved material at 900° C. for 6 h in a N2 atmosphere to obtain a carbon-based material precursor A;
[0069] Step 103, mixing the activated carbon and the carbon-based material precursor A in a mass ratio of 5:5, boiling in a nitric acid solution at 90° C. for 2 hours, cooling and filtering, and washing with pure water until the pH value is 5 to obtain an acid-treated carrier; the mass percentage concentration of the nitric acid solution is 8%, and the mass of the nitric acid solution is 8 times the total mass of the activated carbon and the carbon-based material precursor A;
[0070] Step 104, placing the acid-treated carrier in an ethanol solution of 3% triethylamine by mass, boiling at 100° C. for 2 hours, cooling and filtering, completing the modification, and obtaining a carbon-based material carrier; the mass of the ethanol solution of triethylamine is 9 times the mass of the carrier after acid treatment;
[0071] Step 2: according to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material carrier described in step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol, and stirred at room temperature for 2h for adsorption. During the stirring process, the pH is controlled to 8.5 with a NaOH solution. After the adsorption is completed, the catalyst precursor is obtained by filtering; in the palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.2g / ml, the mass percentage concentration of dimethylaminoethanol is 0.1%, and the mass percentage concentration of the NaOH solution is 5%;
[0072] Step three, placing the catalyst precursor in a reducing agent solution and stirring for reduction to obtain a carbon-based material loaded with precious metal palladium catalyst; the reducing agent solution is a sodium formate solution with a mass percentage concentration of 10%, the stirring reduction temperature is 80°C, and the stirring reduction time is 1h; the mass of the reducing agent solution is 8 times the mass of the catalyst precursor.
[0073] Example 4
[0074] This embodiment provides a method for preparing a carbon-based material-supported noble metal palladium catalyst, wherein the carbon-based material-supported noble metal palladium catalyst is a Pd / C catalyst having a Pd mass percentage of 1%, and the preparation method comprises:
[0075] Step 1: providing a carbon-based material carrier, specifically comprising:
[0076] Step 101, mixing a salt solution, an organic ligand and an alcohol in a mass ratio of 2:50:48, stirring and reacting at 60° C. for 15 hours to obtain a sol; the salt solution is a 0.5 g / ml iron nitrate solution, the organic ligand is pyridazine, and the alcohol is anhydrous ethanol;
[0077] Step 102, drying the sol at 90°C to obtain a gel, crushing the gel and passing it through a 500-mesh sieve, and calcining the sieved material at 700°C for 12 hours under a N2 atmosphere to obtain a carbon-based material precursor A;
[0078] Step 103, mixing the activated carbon and the carbon-based material precursor A in a mass ratio of 5:5, boiling in a nitric acid solution at 90° C. for 2 hours, cooling and filtering, and washing with pure water until the pH value is 5 to obtain an acid-treated carrier; the mass percentage concentration of the nitric acid solution is 8%, and the mass of the nitric acid solution is 8 times the total mass of the activated carbon and the carbon-based material precursor A;
[0079] Step 104, placing the acid-treated carrier in an ethanol solution of 3% triethylamine by mass, boiling at 100° C. for 2 hours, cooling and filtering, completing the modification, and obtaining a carbon-based material carrier; the mass of the ethanol solution of triethylamine is 10 times the mass of the carrier after acid treatment;
[0080] Step 2: according to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material carrier described in step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol, and stirred at room temperature for 2h for adsorption. During the stirring process, the pH is controlled to 8.5 with a NaOH solution. After the adsorption is completed, the catalyst precursor is obtained by filtering; in the palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.2g / ml, the mass percentage concentration of dimethylaminoethanol is 0.1%, and the mass percentage concentration of the NaOH solution is 5%;
[0081] Step three, placing the catalyst precursor in a reducing agent solution and stirring for reduction to obtain a carbon-based material loaded with precious metal palladium catalyst; the reducing agent solution is a sodium formate solution with a mass percentage concentration of 10%, the stirring reduction temperature is 80°C, and the stirring reduction time is 1h; the mass of the reducing agent solution is 8 times the mass of the catalyst precursor.
[0082] Example 5
[0083] This embodiment provides a method for preparing a carbon-based material-supported noble metal palladium catalyst, wherein the carbon-based material-supported noble metal palladium catalyst is a Pd / C catalyst having a Pd mass percentage of 1%, and the preparation method comprises:
[0084] Step 1: providing a carbon-based material carrier, specifically comprising:
[0085] Step 101, mixing a salt solution, an organic ligand and an alcohol in a mass ratio of 2:10:88, stirring and reacting at 60° C. for 15 hours to obtain a sol; the salt solution is a nickel nitrate solution with a mass percentage concentration of 0.5 g / ml, the organic ligand is melamine, and the alcohol is methanol;
[0086] Step 102, drying the sol at 90° C. to obtain a gel, crushing the gel and passing it through a 500-mesh sieve, and calcining the sieved material at 700° C. for 12 h in a N2 atmosphere to obtain a carbon-based material precursor A;
[0087] Step 103, mixing the activated carbon and the carbon-based material precursor A in a mass ratio of 1:9, boiling in a nitric acid solution at 100° C. for 2 h, cooling and filtering, washing with pure water until the pH value is 5, to obtain an acid-treated carrier; the mass percentage concentration of the nitric acid solution is 10%, and the mass of the nitric acid solution is 8 times the total mass of the activated carbon and the carbon-based material precursor A;
[0088] Step 104, placing the acid-treated carrier in an ethanol solution of 3% triethylamine by mass, boiling at 100° C. for 1 hour, cooling and filtering, completing the modification, and obtaining a carbon-based material carrier; the mass of the ethanol solution of triethylamine is 8 times the mass of the carrier after acid treatment;
[0089] Step 2: according to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material carrier described in step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol, and stirred at room temperature for 1.5h for adsorption. During the stirring process, the pH is controlled to 8.5 with a NaOH solution. After the adsorption is completed, the catalyst precursor is obtained by filtering; in the palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.1g / ml, the mass percentage concentration of dimethylaminoethanol is 0.1%, and the mass percentage concentration of the above-mentioned NaOH solution is 5%;
[0090] Step three, placing the catalyst precursor in a reducing agent solution and stirring for reduction to obtain a carbon-based material loaded with precious metal palladium catalyst; the reducing agent solution is a sodium formate solution with a mass percentage concentration of 10%, the stirring reduction temperature is 80°C, and the stirring reduction time is 1h; the mass of the reducing agent solution is 8 times the mass of the catalyst precursor.
[0091] Example 6
[0092] This embodiment provides a method for preparing a carbon-based material-supported noble metal palladium catalyst, wherein the carbon-based material-supported noble metal palladium catalyst is a Pd / C catalyst having a Pd mass percentage of 5%. The preparation method comprises:
[0093] Step 1: providing a carbon-based material carrier, specifically comprising:
[0094] Step 101, mixing a salt solution, an organic ligand and an alcohol in a mass ratio of 2:10:88, stirring and reacting at 60° C. for 15 hours to obtain a sol; the salt solution is a nickel nitrate solution with a mass percentage concentration of 0.5 g / ml, the organic ligand is cyanuric acid, and the alcohol is methanol;
[0095] Step 102, drying the sol at 90° C. to obtain a gel, crushing the gel and passing it through a 400-mesh sieve, and calcining the sieved material at 700° C. for 10 h in a N2 atmosphere to obtain a carbon-based material precursor A;
[0096] Step 103, mixing the activated carbon and the carbon-based material precursor A in a mass ratio of 9:1, boiling in a nitric acid solution at 95° C. for 2 h, cooling and filtering, and washing with pure water until the pH is 5 to obtain an acid-treated carrier; the mass percentage concentration of the nitric acid solution is 8%, and the mass of the nitric acid solution is 8 times the total mass of the activated carbon and the carbon-based material precursor A;
[0097] Step 104, placing the acid-treated carrier in an ethanol solution of 3% triethylamine by mass, boiling at 100° C. for 1.5 hours, cooling and filtering, completing the modification, and obtaining a carbon-based material carrier; the mass of the ethanol solution of triethylamine is 10 times the mass of the carrier after acid treatment;
[0098] Step 2: according to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material carrier described in step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol, and stirred at room temperature for 1h for adsorption. During the stirring process, the pH is controlled to 8.5 with a NaOH solution. After the adsorption is completed, the catalyst precursor is obtained by filtering; in the palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.3g / ml, the mass percentage concentration of dimethylaminoethanol is 0.1%, and the mass percentage concentration of the above-mentioned NaOH solution is 5%;
[0099] Step three, placing the catalyst precursor in a reducing agent solution and stirring for reduction to obtain a carbon-based material loaded with precious metal palladium catalyst; the reducing agent solution is a sodium formate solution with a mass percentage concentration of 10%, the stirring reduction temperature is 80°C, and the stirring reduction time is 1h; the mass of the reducing agent solution is 10 times the mass of the catalyst precursor.
[0100] Example 7
[0101] This embodiment provides a method for preparing a carbon-based material-supported noble metal palladium catalyst, wherein the carbon-based material-supported noble metal palladium catalyst is a Pd / C catalyst having a Pd mass percentage of 1%, and the preparation method comprises:
[0102] Step 1: providing a carbon-based material carrier, specifically comprising:
[0103] Step 101, mixing a salt solution, an organic ligand and an alcohol in a mass ratio of 2:50:48, stirring and reacting at 60° C. for 15 hours to obtain a sol; the salt solution is a 0.5 g / ml iron nitrate solution, the organic ligand is urea, and the alcohol is anhydrous ethanol;
[0104] Step 102, drying the sol at 90° C. to obtain a gel, crushing the gel and passing it through a 500-mesh sieve, and calcining the sieved material at 700° C. for 12 h in a N2 atmosphere to obtain a carbon-based material precursor A;
[0105] Step 103, mixing the activated carbon and the carbon-based material precursor A in a mass ratio of 5:5, boiling in a nitric acid solution at 90° C. for 2 hours, cooling and filtering, and washing with pure water until the pH value is 5 to obtain an acid-treated carrier; the mass percentage concentration of the nitric acid solution is 8%, and the mass of the nitric acid solution is 8 times the total mass of the activated carbon and the carbon-based material precursor A;
[0106] Step 104, placing the acid-treated carrier in an ethanol solution of 3% triethylamine by mass, boiling at 100° C. for 2 hours, cooling and filtering, completing the modification, and obtaining a carbon-based material carrier; the mass of the ethanol solution of triethylamine is 10 times the mass of the carrier after acid treatment;
[0107] Step 2: according to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material carrier described in step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol, and stirred at room temperature for 2h for adsorption. During the stirring process, the pH is controlled to 8.5 with a NaOH solution. After the adsorption is completed, the catalyst precursor is obtained by filtering; in the palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.2g / ml, the mass percentage concentration of dimethylaminoethanol is 0.1%, and the mass percentage concentration of the NaOH solution is 5%;
[0108] Step three, placing the catalyst precursor in a reducing agent solution and stirring for reduction to obtain a carbon-based material loaded with precious metal palladium catalyst; the reducing agent solution is a sodium borohydride solution with a mass percentage concentration of 10%, the stirring reduction temperature is 80°C, and the stirring reduction time is 2h; the mass of the reducing agent solution is 8 times the mass of the catalyst precursor.
[0109] Example 8
[0110] This embodiment provides a method for preparing a carbon-based material-supported noble metal palladium catalyst, wherein the carbon-based material-supported noble metal palladium catalyst is a Pd / C catalyst having a Pd mass percentage of 3%. The preparation method comprises:
[0111] Step 1: providing a carbon-based material carrier, specifically comprising:
[0112] Step 101, mixing a salt solution, an organic ligand and an alcohol in a mass ratio of 10:50:40, stirring and reacting at 100° C. for 8 hours to obtain a sol; the salt solution is a solution containing iron nitrate and copper nitrate, the mass percentage concentration of the copper nitrate solution and the iron nitrate solution in the solution containing iron nitrate and copper nitrate is both 0.5 g / ml, the organic ligand is thiourea and urea in a mass ratio of 1:1, and the alcohol is methanol;
[0113] Step 102, drying the sol at 150°C to obtain a gel, crushing the obtained gel and passing it through a 350-mesh sieve, and calcining the sieved material at 800°C for 8h under a N2 atmosphere to obtain a carbon-based material precursor A;
[0114] Step 103, mixing the activated carbon and the carbon-based material precursor A in a mass ratio of 7:3, boiling in a nitric acid solution at 90° C. for 2 h, cooling and filtering, and washing with pure water until the pH is 5 to obtain an acid-treated carrier; the mass percentage concentration of the nitric acid solution is 5%, and the mass of the nitric acid solution is 10 times the total mass of the activated carbon and the carbon-based material precursor A;
[0115] Step 104, placing the acid-treated carrier in an ethanol solution with a mass percentage concentration of 3% triethylamine, boiling at 90° C. for 2 hours, cooling and filtering, completing the modification, and obtaining a carbon-based material carrier; the mass of the ethanol solution of triethylamine is 10 times the mass of the carrier after acid treatment;
[0116] Step 2: according to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material carrier described in step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol, and stirred at room temperature for 3h for adsorption. During the stirring process, the pH is controlled to 8.5 with a NaOH solution. After the adsorption is completed, the catalyst precursor is obtained by filtering; in the palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.2g / ml, the mass percentage concentration of dimethylaminoethanol is 0.2%, and the mass percentage concentration of the above-mentioned NaOH solution is 5%;
[0117] Step three, placing the catalyst precursor in a reducing agent solution and stirring for reduction to obtain a carbon-based material loaded with precious metal palladium catalyst; the reducing agent solution is a sodium formate solution with a mass percentage concentration of 20%, the stirring reduction temperature is 90°C, and the stirring reduction time is 2h; the mass of the reducing agent solution is 10 times the mass of the catalyst precursor.
[0118] Example 9
[0119] This embodiment provides a method for preparing a carbon-based material-supported noble metal palladium catalyst, wherein the carbon-based material-supported noble metal palladium catalyst is a Pd / C catalyst having a Pd mass percentage of 5%. The preparation method comprises:
[0120] Step 1: providing a carbon-based material carrier, specifically comprising:
[0121] Step 101, mixing a salt solution, an organic ligand and an alcohol in a mass ratio of 10:50:40, stirring and reacting at 100° C. for 8 hours to obtain a sol; the salt solution is a solution containing iron nitrate and nickel nitrate, the mass percentage concentration of the copper nitrate solution and the iron nitrate solution in the solution containing iron nitrate and nickel nitrate is 0.5 g / ml, the organic ligand is urea, melamine and cyanuric acid in a mass ratio of 2:1:1, and the alcohol is methanol;
[0122] Step 102, drying the sol at 150°C to obtain a gel, crushing the obtained gel and passing it through a 350-mesh sieve, and calcining the sieved material at 800°C for 8h under a N2 atmosphere to obtain a carbon-based material precursor A;
[0123] Step 103, mixing the activated carbon and the carbon-based material precursor A in a mass ratio of 7:3, boiling in a nitric acid solution at 90° C. for 2 h, cooling and filtering, and washing with pure water until the pH is 5 to obtain an acid-treated carrier; the mass percentage concentration of the nitric acid solution is 5%, and the mass of the nitric acid solution is 10 times the total mass of the activated carbon and the carbon-based material precursor A;
[0124] Step 104, placing the acid-treated carrier in an ethanol solution with a mass percentage concentration of 3% triethylamine, boiling at 90° C. for 2 hours, cooling and filtering, completing the modification, and obtaining a carbon-based material carrier; the mass of the ethanol solution of triethylamine is 8 times the mass of the carrier after acid treatment;
[0125] Step 2: according to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material carrier described in step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol, and stirred at room temperature for 3h for adsorption. During the stirring process, the pH is controlled to 8.5 with a NaOH solution. After the adsorption is completed, the catalyst precursor is obtained by filtering; in the palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.2g / ml, the mass percentage concentration of dimethylaminoethanol is 0.2%, and the mass percentage concentration of the above-mentioned NaOH solution is 5%;
[0126] Step three, placing the catalyst precursor in a reducing agent solution and stirring for reduction to obtain a carbon-based material loaded with precious metal palladium catalyst; the reducing agent solution is a sodium formate solution with a mass percentage concentration of 20%, the stirring reduction temperature is 90°C, and the stirring reduction time is 1 hour; the mass of the reducing agent solution is 8 times the mass of the catalyst precursor.
[0127] Comparative Example 1
[0128] The present comparative example provides a method for preparing a Pd / C catalyst, comprising: stirring and mixing a palladium nitrate solution and activated carbon for 1 hour according to a preset Pd mass percentage content of 5% in the Pd / C catalyst, introducing sodium formate into the stirred and mixed system, stirring and reducing for 1 hour, washing, and filtering to obtain a Pd / C catalyst.
[0129] Comparative Example 2
[0130] The preparation method of the catalyst of this comparative example refers to Example 4 of patent CN117085700A.
[0131] Application Example 1.1
[0132] This application example provides a method for catalytically synthesizing 5-pyrimidinecarboxaldehyde using the catalysts of Examples 1 to 9 and Comparative Examples 1 and 2 as dechlorination catalysts, wherein the raw materials include: 4,6-dichloro-5-pyrimidinecarboxaldehyde, methanol, a Pd / C catalyst and sodium bicarbonate, wherein the mass percentage of Pd in the Pd / C catalyst is 5%, and the mass ratio of the 4,6-dichloro-5-pyrimidinecarboxaldehyde, methanol, Pd / C catalyst and sodium bicarbonate is 5:75:0.1:1; in the catalytic synthesis of 5-pyrimidinecarboxaldehyde, the hydrogen pressure is 1.5 MPa, the reaction temperature is 70°C, the reaction time is 6 h, the reaction speed is 900 r / min, and the purity of the product in the system after the reaction is analyzed by chromatography, and the results are shown in Table 2.
[0133] Table 2 5-pyrimidinecarboxaldehyde catalytic synthesis reaction results
[0134]
[0135] As can be seen from Table 2, the dechlorination reaction catalyst prepared by the method of the present invention can achieve a product purity of up to 94.6% in the synthesis of 5-pyrimidinecarboxaldehyde. The catalyst prepared by the method of the present invention is significantly higher than the traditional catalyst (Comparative Example 1); and the performance of the catalyst prepared by referring to Example 4 of patent CN117085700A is slightly better (Comparative Example 2).
[0136] Application Example 1.2
[0137] This application example provides a method for catalytically synthesizing 5-pyrimidinecarboxaldehyde under sulfur poisoning conditions using the catalysts of Example 2 and Comparative Example 2. The raw materials include sodium sulfide in addition to those in Application Example 1.1. The mass ratio of sodium sulfide to catalyst is 1:330. The results are shown in Table 3.
[0138] Table 3 Catalytic synthesis of 5-pyrimidinecarboxaldehyde under sulfur poisoning conditions
[0139]
[0140]
[0141] It can be seen from Table 3 that the catalyst of the present invention can avoid poisoning and maintain high reaction activity.
[0142] Application Example 1.3
[0143] This application example provides a method for catalytically synthesizing 5-pyrimidinecarboxaldehyde using the catalysts of Example 2 and Comparative Example 2. The application method is the same as that of Application Example 1.1. Each time the catalyst is applied, no treatment is done on the catalyst after the previous use. The data are as follows.
[0144] Table 4 Catalytic synthesis of 5-pyrimidinecarboxaldehyde using catalysts
[0145]
[0146] According to Table 4, the catalyst of the present invention can be used twice in the reaction of synthesizing 5-pyrimidinecarboxaldehyde while still maintaining high product purity, and the reaction activity and stability of the catalyst are significantly better than those of the comparative example.
[0147] Application Example 2.1
[0148] This application example provides a method for catalytically synthesizing 2,3-dichloropyridine using the catalysts of Examples 1 to 9 and Comparative Examples 1 and 2 as dechlorination catalysts, wherein the raw materials include: 2,3,4,5-tetrachloropyridine, methanol, triethylamine and Pd / C catalyst, and the mass ratio of 2,3,4,5-tetrachloropyridine, methanol, triethylamine and Pd / C catalyst is 25:80:15:0.05 according to the mass percentage of Pd in the Pd / C catalyst being 3%; in the catalytic synthesis of 2,3-dichloropyridine, the hydrogen pressure is 1.0 MPa, the reaction temperature is 45°C, the reaction time is 6 hours, and the reaction speed is 900 r / min. The purity of the product in the system after the reaction is analyzed by chromatography, and the results are shown in Table 5.
[0149] Table 5 Catalytic synthesis of 2,3-dichloropyridine reaction results
[0150]
[0151] According to Table 5, the dechlorination reaction catalyst prepared by the method of the present invention can achieve a product purity of up to 65.8% in the catalytic synthesis of 2,3-dichloropyridine, and the catalyst prepared by the method of the present invention is significantly higher than the comparative example.
[0152] Application Example 2.2
[0153] This application example provides a method for catalytically synthesizing 2,3-dichloropyridine under sulfur poisoning conditions using the catalysts of Example 2 and Comparative Example 2. The raw materials include sodium sulfide in addition to those of Application Example 2.1. The mass ratio of sodium sulfide to the catalyst is 1:250. The results are shown in Table 6.
[0154] Table 6 Catalytic synthesis of 2,3-dichloropyridine under sulfur poisoning conditions
[0155]
[0156]
[0157] It can be seen from Table 6 that the catalyst of the present invention can avoid poisoning and maintain high reaction activity.
[0158] Application Example 2.3
[0159] This application example provides a method for catalytically synthesizing 2,3-dichloropyridine using the catalysts of Example 2 and Comparative Example 2. The application method is the same as that of Application Example 2.1. Each time the catalyst is applied, no treatment is done on the catalyst after the last use. The data are as follows.
[0160] Table 7 Catalytic synthesis of 2,3-dichloropyridine using catalysts
[0161]
[0162] According to Table 7, the catalyst of the present invention can be used four times in the synthesis of 2,3-dichloropyridine while still maintaining high product purity, and the reaction activity and stability of the catalyst are significantly better than those of the comparative example.
[0163] Combining Application Examples 1 and 2, it can be seen that the dechlorination reaction catalyst of the present invention exhibits excellent catalytic ability in catalytic dechlorination reaction, which is manifested in the obvious improvement of the purity of the upper product in the synthesis of 5-pyrimidinecarboxaldehyde and the synthesis of 2,3-dichloropyridine.
[0164] Application Example 3
[0165] This application example provides a method for catalytically synthesizing biotin using the catalysts of Examples 1 to 2 and Comparative Examples 1 to 2 as dechlorination catalysts, wherein the raw materials include: D-biotin intermediate, methanol, and Pd / C catalyst, wherein the mass ratio of the D-biotin intermediate, methanol, and Pd / C catalyst is 5:13:0.05 based on the mass percentage of Pd in the Pd / C catalyst being 5%; in the catalytic synthesis of D-biotin, the hydrogen pressure is 4.5 MPa, the reaction temperature is 110°C, the reaction time is 3 h, and the reaction speed is 600 r / min. The purity of the product in the system after the reaction is analyzed by chromatography, and the results are shown in Table 8.
[0166] Table 8 Catalytic synthesis of biotin
[0167]
[0168] According to Table 8, the reaction substrate in the catalytic synthesis of biotin contains sulfur atoms, which has a certain poisoning effect on the catalyst. When the catalyst of the present invention is used to catalyze the synthesis of biotin, the product purity still exceeds 93%, which is significantly higher than the comparative example. Combined with Application Examples 1 to 3, it can be seen that the catalyst of the present invention has excellent resistance to the poisoning effect of the raw material itself and the poisoning during the reaction process.
[0169] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing a carbon-based material-supported noble metal palladium catalyst, characterized in that: include: Step 1: providing a carbon-based material carrier, specifically comprising: Step 101, mixing a salt solution, an organic ligand and an alcohol in a mass ratio of (2-15):(10-50):(35-88), stirring and reacting at 60-100° C. for 8-15 hours to obtain a sol; Step 102, drying the sol at 90-150° C. to obtain a gel, crushing the obtained gel and passing it through a 300-500 mesh sieve, and calcining the sieved material at 600-900° C. for 6-12 hours under a N2 atmosphere to obtain a carbon-based material precursor A; Step 103, mixing the activated carbon and the carbon-based material precursor A in a mass ratio of (1-9):(9-1), cooking in a nitric acid solution at 90° C. to 100° C. for 1 h to 2 h, cooling, filtering, and washing to obtain an acid-treated carrier; Step 104, placing the acid-treated carrier in an ethanol solution of triethylamine, cooking at 90° C. to 100° C. for 1 h to 2 h, cooling and filtering to complete the modification and obtain a carbon-based material carrier; Step 2: according to the preset palladium mass percentage in the Pd / C catalyst, the carbon-based material carrier described in step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol, stirred at room temperature for 1 to 3 hours for adsorption, and filtered to obtain a catalyst precursor; Step 3: placing the catalyst precursor in a reducing agent solution and stirring for reduction to obtain a carbon-based material-loaded noble metal palladium catalyst.
2. The method for preparing a carbon-based material-supported noble metal palladium catalyst according to claim 1, characterized in that: The carbon-based material-loaded noble metal palladium catalyst is a Pd / C catalyst with a Pd mass percentage of 1% to 5%.
3. The method for preparing a carbon-based material-supported noble metal palladium catalyst according to claim 1, characterized in that: In step 101, the salt solution is a metal-soluble salt solution, the organic ligand is one or more of dicyandiamide, thiourea, pyridazine, melamine, cyanuric acid and urea, and the alcohol is methanol or anhydrous ethanol.
4. The method for preparing a carbon-based material-supported noble metal palladium catalyst according to claim 3, characterized in that: The metal soluble salt is one or more of ferric nitrate, copper nitrate and nickel nitrate.
5. The method for preparing a carbon-based material-supported noble metal palladium catalyst according to claim 1, characterized in that: In step 103, the mass percentage concentration of the nitric acid solution is 5% to 10%, and the mass of the nitric acid solution is 8 to 10 times the total mass of the activated carbon and the carbon-based material precursor A.
6. The method for preparing a carbon-based material-supported noble metal palladium catalyst according to claim 1, characterized in that: In step 104, the mass percentage concentration of the triethylamine ethanol solution is 3%, and the mass of the triethylamine ethanol solution is 8 to 10 times the mass of the acid-treated carrier.
7. The method for preparing a carbon-based material-supported noble metal palladium catalyst according to claim 1, characterized in that: In step 2, in the palladium nitrate solution containing dimethylaminoethanol, the concentration of palladium nitrate is 0.1 g / ml to 0.5 g / ml, and the mass percentage concentration of dimethylaminoethanol is 0.1% to 0.3%.
8. The method for preparing a carbon-based material-supported noble metal palladium catalyst according to claim 1, characterized in that: In step three, the reducing agent solution is sodium formate solution or sodium borohydride solution, with a mass percentage concentration of 10% to 20%, the stirring reduction temperature is 80°C to 90°C, the stirring reduction time is 1h to 2h, and the mass of the reducing agent solution is 8 to 10 times the mass of the catalyst precursor.
9. The method for preparing a carbon-based material-supported noble metal palladium catalyst according to claim 1, characterized in that: Step 2 also includes controlling the pH of the system to 8.5 during the adsorption process.
10. A dechlorination catalyst, characterized in that: The dechlorination catalyst is prepared by the method for preparing a carbon-based material-supported noble metal palladium catalyst according to claim 1.
Citation Information
Patent Citations
Catalyst for selective hydrogenation reaction of aromatic nitrocompound and preparation method of catalyst
CN105032424A
Carbon-palladium carbon catalyst mixture and preparation method thereof
CN108031469A
Preparation method of supported catalyst for synthesizing chloroaniline through catalytic hydrogenation of chloronitrobenzene
CN109939713A
Catalyst for hydrodechlorination of chlorinated aromatic hydrocarbon as well as preparation method and application of catalyst
CN114367296A
Aza-carbon-based supported metal catalyst as well as preparation method and application thereof
CN114984994A
Cited By
Preparation method of N-(5-pyrimidinemethyl)-2-pyridylamine
CN120842201A