Preparation method and application of three-dimensional ordered macroporous catalytic filter material

By combining the three-dimensional ordered macroporous catalyst MnCeTiOx with polytetrafluoroethylene calendered film and combined with ultraviolet light assisted technology, the problem of catalyst coverage and loss is solved, and the treatment efficiency of antibiotic wastewater and the utilization rate of catalyst are improved.

CN118988416AActive Publication Date: 2024-11-22RES INST OF ZHEJIANG UNIV TAIZHOU

Patent Information

Application Number
CN202411250074.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-22
Estimated Expiration
2044-09-06

AI Technical Summary

Technical Problem

When existing catalytic materials treat antibiotic wastewater, photogenerated electrons and holes are difficult to separate, and the catalyst is easily covered and lost by particulate matter, resulting in low catalytic efficiency and short service life.

Method used

The three-dimensional ordered macroporous catalyst MnCeTiOx is used to combine with the polytetrafluoroethylene calendered film to enhance the bonding strength between the catalyst and the filter cloth through the binder, and use ultraviolet light to generate strong oxidative radicals to assist catalytic degradation to avoid the catalyst being wrapped and lost. .

Benefits of technology

It improves the utilization rate and catalytic activity of the catalyst, extends the service life, enhances the coordinated removal efficiency of sewage organic matter and particulate matter, and improves the low-temperature catalytic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988416A_ABST
    Figure CN118988416A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a three-dimensional ordered macroporous catalytic filter material, preparation of a catalyst comprises the steps of preparation of a mixed solution, preparation of a colloidal crystal template and removal of the colloidal crystal template, and the prepared three-dimensional ordered macroporous MnCeTiOx catalyst effectively relieves the problem that particles cover active sites of the catalyst. The regulation and control of surface acidic sites and active sites are realized by utilizing the intermetallic interaction of Mn, Ce and Ti, so that the low-temperature catalytic performance is effectively improved; the surface of a PTFE rolled film is coated with a layer of thin binder, the binder is used as a connecting bridge, loading is carried out in a spraying mode, and the three-dimensional ordered macroporous catalytic filter material in which a catalyst and the filter material are firmly combined is formed through the steps of stretching, slitting, curling, needling and the like. According to the filter cloth, the condition that a catalyst is covered by particulate matters in the using process is relieved through a three-dimensional ordered macroporous structure, the bonding strength of the catalyst and the filter cloth is enhanced through the bonding agent, and the problems of catalyst loss, catalyst wrapping and the like are relieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water pollution remediation, and in particular to a preparation method and application of a three-dimensional ordered macroporous catalytic filter material. Background Art

[0002] In recent years, various new pollutants have emerged one after another, the most typical of which is antibiotic wastewater, which mainly comes from hospitals, pharmaceutical industry, livestock industry, aquaculture and other fields. Antibiotic wastewater has biological toxicity, environmental persistence and accumulation. Catalytic oxidation technology has the advantages of high efficiency, mild reaction conditions, stability, green and pollution-free, etc., and has received widespread attention in recent years in the treatment of new pollutants in water. However, existing catalytic materials have some shortcomings in actual use: (1) It is difficult to separate the photogenerated electrons and holes of traditional catalytic materials, and they are very easy to recombine during the reaction process, which greatly affects the catalytic efficiency; (2) Catalytic materials are easy to lose during the treatment process and have a short service life. For this reason, catalytic filter materials that integrate catalysis and filtration functions have come into being, which can achieve compactness of equipment while completing pollutant removal.

[0003] The photocatalytic nanofiber membrane provided by patent CN117599834B "A photocatalytic nanofiber membrane and its preparation method and application" can adsorb tetracycline antibiotic pollutants to the surface of the membrane material and the inside of the pores for catalytic degradation, thereby improving the treatment efficiency of tetracycline antibiotics. However, the catalyst is wrapped by the fiber, which reduces the catalyst utilization rate. Patent CN116835749A "A photocatalytic hydrogel material treatment device for antibiotic wastewater degradation" provides a photocatalytic hydrogel material and a photocatalytic treatment process device applied to antibiotic wastewater, which can effectively utilize the light source to achieve efficient treatment of antibiotic wastewater, but requires additional equipment, and particulate matter in the sewage will block / cover the catalyst active sites and reduce the catalytic activity. Therefore, it is necessary to develop a new catalytic filter material preparation technology to overcome the problems of catalyst loss with the movement of the fluid and catalyst active sites being blocked during use. Summary of the invention

[0004] In order to solve at least one of the above problems, the present invention provides a preparation method and application of a three-dimensional ordered macroporous catalytic filter material. The catalytic filter material prepared by the method of the present invention alleviates the problem of the catalyst being covered by particulate matter during use with a three-dimensional ordered macroporous structure, and strengthens the bonding strength between the catalyst and the filter cloth with a binder, thereby alleviating the problems of catalyst loss and catalyst being wrapped, and can ensure the synergistic removal efficiency of sewage organic matter and particulate matter.

[0005] In order to achieve the above-mentioned object, the present invention adopts the following technical means: The first aspect of the present invention provides a method for preparing a three-dimensional ordered macroporous catalyst, comprising the following steps:

[0006] (1) Preparation of mixed solution

[0007] First, add the complexing agent to the mixed solution of methanol and ethylene glycol, stir in a water bath at 60-80℃ for 1-2h, and then cool to room temperature. Next, add the precursor solution to the above solution, continue stirring at 40-50℃ for 1-2h to ensure that the solution is mixed evenly; the complexing agent accounts for 1-5wt% of the mixed solution, and the precursor solution accounts for 20-60wt% of the mixed solution

[0008] (2) Preparation of colloidal crystal templates

[0009] The organic polymer nanospheres are immersed in the above solution for 4-6 hours. After the organic polymer nanospheres are thoroughly immersed, the excess metal precursor solution is filtered using a vacuum funnel to obtain a colloidal crystal template, which is then placed in a vacuum oven at 40-50° C. and dried for 48-50 hours.

[0010] (3) Colloidal crystal template removal

[0011] The colloidal crystal template is removed by calcination. The calcination process is as follows:

[0012] (A) Pretreatment: Dry the sample at 80-100 ml min -1 The calcination was carried out in a calcination atmosphere at a temperature of 1-3 °C·min -1 The rate is raised from room temperature to 300-350°C, maintained for 4-5h, and then cooled to room temperature;

[0013] (B) Template removal: The pretreated sample was at 80-100 ml min -1 The calcination was carried out in a calcination atmosphere at a temperature of 1-3 °C·min -1 The temperature was raised from room temperature to 500-550℃ and maintained at 500-550℃ for 5-6h. The catalyst was cooled to obtain a three-dimensional ordered macroporous MnCeTiO x catalyst;

[0014] In some embodiments of the present invention, in step (1), the complexing agent is one or more of oxalic acid and citric acid.

[0015] In some embodiments of the present invention, the precursor solution in step (1) comprises a manganese species, a cerium species and titanium dioxide, the manganese species may be one of manganese nitrate, manganese chloride or manganese acetate, the cerium species may be one of cerium nitrate, cerium sulfate or cerium acetate,

[0016] In some embodiments of the present invention, the precursor solution is a mixed solution of cerium nitrate, manganese nitrate and titanium dioxide in a mass ratio of (1-4):(1-4):(20-30). Preferably, the mass ratio of cerium nitrate, manganese nitrate and titanium dioxide in the mixed solution is 4:4:20.

[0017] In some embodiments of the present invention, the organic polymer nanospheres in step (2) are one of polystyrene, polymethyl methacrylate and porous silicon microspheres. In some embodiments of the present invention, preferably, the organic polymer nanospheres are polymethyl methacrylate.

[0018] In some embodiments of the present invention, the calcination atmosphere in step (3) is nitrogen or air.

[0019] The present invention also provides a catalyst prepared by the method described in the first aspect and use of the catalyst in preparing a catalytic filter material product for removing organic matter and particulate matter from water.

[0020] The second aspect of the present invention provides a method for preparing a three-dimensional ordered macroporous catalytic filter material, comprising the following steps:

[0021] (1) Preparation of three-dimensional ordered macroporous MnCeTiO x catalyst

[0022] The three-dimensional ordered macroporous MnCeTiO x catalyst;

[0023] (2) Preparation of polytetrafluoroethylene (PTFE) calendered film

[0024] The polytetrafluoroethylene resin and the auxiliary agent are uniformly mixed in a weight ratio of (2-4): (0.1-1), and allowed to stand at 80° C. for 12-24 hours to promote the auxiliary agent and the polytetrafluoroethylene resin to be fully mixed and form a material, and then the mixed material is calendered at a temperature of 40 to 80° C. to obtain a PTFE calendered film;

[0025] (3) Preparation of catalytic filter material

[0026] A thin layer of adhesive is applied on the surface of the PTFE calendered membrane, and then the catalyst is loaded on the PTFE calendered membrane by spraying using the adhesive as a connecting bridge. Finally, the catalytic filter material is prepared through the steps of stretching, slitting, curling and needle punching.

[0027] In some embodiments of the present invention, the auxiliary agent in step (2) may be one of kerosene, liquid paraffin or petroleum ether.

[0028] In some embodiments of the present invention, the binder in step (3) may be one of coal tar, organic titanium coupling agent or epoxy resin adhesive.

[0029] The third aspect of the present invention provides a catalytic filter material prepared according to the method described in the second aspect.

[0030] The use of the catalytic filter material prepared by the method described in the first aspect and the catalytic filter material described in the second aspect in the preparation of products for removing organic matter and particulate matter from water bodies; in some embodiments, the application is combined with ultraviolet light, and ultraviolet light and its strong oxidizing free radicals are used to assist the catalyst in degrading organic matter in wastewater, thereby further improving the catalytic performance.

[0031] Beneficial effects of the present invention

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The present invention provides a catalyst - three-dimensional ordered macroporous MnCeTiO x The catalyst is used as the catalytic active component of the catalytic filter material. The three-dimensional ordered macroporous structure effectively alleviates the problem of particle accumulation on the catalyst surface. The metal interaction between Mn, Ce and Ti is used to achieve the regulation of surface acidic sites and active sites, effectively improving the catalytic performance at low temperatures. Among them, the multivalent and low-temperature highly active metal Mn is the main active phase.

[0034] (2) The catalytic filter material of the present invention combines the catalyst with the filter cloth by using a binder, so that the catalyst is present on the fiber surface, thereby enhancing the bonding strength between the catalyst and the filter cloth; at the same time, the problem of the catalyst being wrapped in the blending drawing method, which affects the physical properties of the filter cloth, is avoided. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 A flow chart for preparing catalytic filter material is shown;

[0036] Figure 2 The schematic diagram of the structure of the organic matter catalytic device for sewage is shown;

[0037] Among them, 1. feed tank, 2. peristaltic pump, 3. catalytic filter, 4. UV lamp, 5. sampling port. DETAILED DESCRIPTION

[0038] The present invention discloses a preparation method and application of a three-dimensional ordered macroporous catalytic filter material, which can be used to remove water pollutants and particulate matter. The specific preparation steps of the catalytic filter material are as follows: Figure 1 As shown below:

[0039] The catalyst is prepared through the steps of mixed solution preparation, colloidal crystal template synthesis, colloidal crystal template removal, PTFE calendering film preparation and catalytic filter material preparation to form a catalytic filter material in which the catalyst and the filter cloth are firmly combined.

[0040] In actual use, the prepared filter cloth allows wastewater to flow through the pores of the catalytic filter material through a peristaltic pump, thereby strengthening the mass transfer between the catalyst and the wastewater. At the same time, ultraviolet light and the strong oxidizing free radicals it produces are used to assist the catalyst in degrading organic matter in the wastewater and improve the catalytic performance. Ultraviolet light is used to promote the generation of photogenerated electrons on the catalyst surface, thereby improving the degradation efficiency. At the same time, strong oxidizing free radicals such as ozone are generated to promote degradation. The required wavelength of ultraviolet light is: 254nm.

[0041] The composite catalytic filter material is Figure 2 The catalytic device shown includes a feed tank 1 connected in sequence, a peristaltic pump 2 connected to a catalytic filter material filter 3, a catalytic filter material and an ultraviolet lamp 4 installed in the catalytic filter material filter 3, and a sampling port 5 is provided at the lower end of the catalytic filter material filter 3.

[0042] The above device was tested for antibiotic wastewater treatment at a constant pressure of 0.2Mpa. The test process is as follows:

[0043] The catalytic filter material to be tested is installed in the catalytic filter material device, the ultraviolet lamp 4 is turned on, 1.2L of untreated sewage is added to the feed tank, and then the peristaltic pump 2 and gravity are used to circulate the sewage between the feed tank 1 and the catalytic filter material filter 3. The circulation treatment time is 30 minutes. During the test, samples are collected through the sampling port 5.

[0044] The catalyst content and loss of the catalytic filter material are tested by weighing the filter cloth before and after use.

[0045] The technical solution of this patent is further described in detail below in conjunction with specific implementation methods.

[0046] Example 1

[0047] The specific preparation steps of the catalytic filter material of this embodiment are as follows:

[0048] (1) Preparation of mixed solution

[0049] First, add the complexing agent oxalic acid to the mixed solution of methanol and ethylene glycol, stir in a 70℃ water bath for 1h, and then cool to room temperature. Next, add the precursor solution to the above solution, continue stirring at 40℃ for 1h to ensure that the solution is evenly mixed. The mass ratio of cerium nitrate, manganese nitrate, and titanium dioxide in the precursor solution is 4:4:20; the complexing agent accounts for 3wt% of the mixed solution, and the precursor solution accounts for 50wt% of the mixed solution.

[0050] (2) Preparation of colloidal crystal templates

[0051] The polymethyl methacrylate nanospheres were immersed in the above solution for 4 h. After the polymethyl methacrylate nanospheres were thoroughly immersed, the excess metal precursor solution was filtered using a vacuum funnel to obtain a colloidal crystal template, which was then placed in a vacuum oven at 50° C. and dried for 48 h.

[0052] (3) Colloidal crystal template removal

[0053] The colloidal crystal template is removed by calcination; the calcination process is as follows:

[0054] (A) Pretreatment: Dry the sample at 80 ml min -1 The calcination was carried out in a nitrogen atmosphere at a temperature of 1 °C·min -1 The temperature was raised from room temperature to 310 °C at a rate of 40 °C, maintained for 4 h, and then cooled to room temperature;

[0055] (B) Template removal: The pretreated sample was heated at 80 ml min -1 The calcination was carried out in a nitrogen atmosphere at a temperature of 1 °C·min -1 The temperature was raised from room temperature to 550℃ and maintained at 550℃ for 5h. Then, the temperature was lowered to room temperature to obtain three-dimensional ordered macroporous MnCeTiO x catalyst.

[0056] (4) Preparation of PTFE calendered membrane

[0057] The aviation kerosene and the PTFE resin were uniformly mixed in a weight ratio of 0.5:4, and allowed to stand at 80°C for 12 hours to promote the auxiliary agent and the polytetrafluoroethylene resin to mix fully and form a material, and then the mixed material was calendered at 80°C to obtain a PTFE calendered film.

[0058] (5) Preparation of catalytic filter material

[0059] A thin layer of epoxy resin adhesive is applied on the surface of the PTFE calendering film, and then the catalyst is loaded on the PTFE calendering film by spraying using the epoxy resin adhesive as a connecting bridge. The spraying amount is 5wt% of the calendering film. Finally, the catalytic filter material is prepared by stretching, slitting, curling and acupuncture.

[0060] The catalyst content of the PTFE catalytic filter material prepared by the above method is 33.1 g / m 2 .

[0061] Example 2

[0062] The steps for preparing the catalytic filter material in this embodiment are similar to those in embodiment 1, except that the catalyst spraying amount in step (5) is increased to 15 wt %. The catalyst content of the PTFE catalytic filter material prepared by the above method is 103.5 g / m 2 .

[0063] Example 3

[0064] The steps for preparing the catalytic filter material in this embodiment are similar to those in Example 1, except that the catalyst spraying amount in step (5) is increased to 30 wt %. The catalyst content of the PTFE catalytic filter material prepared by the above method is 215.6 g / m 2 .

[0065] Example 4

[0066] The steps for preparing the catalytic filter material in this embodiment are similar to those in Example 1, except that the ratio of the precursor solution in step (1) is adjusted, wherein the mass ratio of cerium nitrate, manganese nitrate, and titanium dioxide is 4:4:15. The catalyst content of the PTFE catalytic filter material prepared by the above method is 216.4 g / m 2 .

[0067] Example 5

[0068] The steps for preparing the catalytic filter material in this embodiment are similar to those in embodiment 1, except that the ratio of the precursor solution in step (1) is adjusted, wherein the mass ratio of cerium nitrate, manganese nitrate, and titanium dioxide is 4:4:25. The catalyst content of the PTFE catalytic filter material prepared by the above method is 212.9 g / m 2 .

[0069] Comparative Example 1

[0070] The difference from Example 3 is that this example adopts the blending wire drawing method to prepare the catalytic filter material:

[0071] In step (4) and step (5), the three-dimensional ordered macroporous catalyst, aviation kerosene, and PTFE resin are uniformly mixed in a weight ratio of 0.4:0.5:4, and then the catalytic filter material is prepared by extrusion, calendaring, stretching, needle puncture, etc. The catalyst content of the PTFE catalytic filter material prepared by the above method is 204.2 g / m 2 .

[0072] The catalytic filter materials prepared in Examples 1-5 and Comparative Examples 1-2 were placed in a catalytic device, the ultraviolet lamp was turned on, and the performance of the catalytic filter materials was analyzed at a flow rate of 200 ml / min and a tetracycline concentration of 5.0 mg / L in wastewater.

[0073] After the test started, samples were taken every 10 minutes and measured for 60 minutes. The average value was recorded as the COD removal rate. The measurement was repeated 6 times and the COD removal rate and catalyst loss were recorded. The results are shown in Tables 1 and 2 below.

[0074] Table 1 COD removal rates of Examples 1-5 and Comparative Example 1

[0075]

[0076] It can be seen from Table 1 that the catalytic filter material preparation parameters adopted in Example 3 are the optimal conditions, which well solve the problem of the accumulation of particulate matter on the filter material surface inhibiting the COD removal efficiency. The catalytic filter material in this application has a high removal capacity for sewage COD.

[0077] Table 2 Particle removal rates of Examples 1-5 and Comparative Example 1

[0078]

[0079] It can be seen from Table 2 that the catalytic filter material prepared in the above example still has a high particle removal capacity after recycling.

[0080] By comparing Examples 1-3, it can be seen that the catalyst spraying amount has a great influence on the COD removal rate, and the catalyst spraying amount of Example 3 has the highest COD removal performance.

[0081] When the catalyst spraying amount is higher, the initial catalyst COD removal rate will increase appropriately, but the catalyst is easy to be lost during use, and the removal rate will decrease due to catalyst loss after use.

[0082] By comparing Examples 3-5, it can be seen that there is a suitable ratio between the metal contents in the filter material, which can effectively improve the interaction between Mn, Ce and Ti. The COD removal rates are as follows from large to small: Example 3 (Ti: 20) > Example 4 (Ti: 15) > Example 5 (Ti: 25).

[0083] As can be seen from the figure, the catalyst of Comparative Example 1 is partially coated with PTFE, so that its COD removal performance is significantly reduced compared with Example 3, while the catalyst of Example 3 mainly exists on the PTFE surface, which can effectively avoid the influence of catalyst addition on the physical properties of the filter material.

[0084] The changes in catalyst content of the catalytic filter material are shown in Table 3.

[0085] Table 3 Changes in catalyst content of catalytic filter material

[0086] Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 <![CDATA[0th (g / m 2 )]]> 33.1 103.5 215.6 216.4 212.9 204.2 <![CDATA[6th (g / m 2 )]]> 30.1 97.8 210.5 212.5 206.7 185.6 <![CDATA[Catalyst loss amount (g / m 2 )]]> 3.1 5.7 5.1 3.9 6.2 18.6

[0087] By comparing Examples 1-3, it can be seen that the catalyst spraying amount has a great influence on the catalyst content, and the catalyst spraying amount of Example 3 has the highest catalyst loading.

[0088] Comparing Example 3 with Comparative Example 1, the catalytic filter material prepared in Comparative Example 1 has a large amount of catalyst loss during use, while the binder used in Examples 1-3 can effectively improve the bonding strength between the catalyst and the filter material, and reduce the catalyst loss of the catalytic filter material during use.

[0089] The present invention is not limited to the above-mentioned embodiments. On the basis of the technical solution disclosed in the present invention, technicians in this field may make some substitutions and improvements to some technical features therein according to the disclosed technical content without departing from the principles of the present invention. These substitutions and improvements should also be regarded as within the protection scope of the present invention.

Claims

1. A method for preparing a three-dimensional ordered macroporous catalytic filter material, characterized in that: The steps include: (1) Preparation of mixed solution Adding the complexing agent to a mixed solution of methanol and ethylene glycol, stirring in a water bath, and cooling to room temperature; adding the precursor solution to the above solution, and continuing to stir evenly to obtain a mixed solution, wherein the complexing agent accounts for 1-5wt% of the mixed solution, and the precursor solution accounts for 20-60wt% of the mixed solution; (2) Preparation of colloidal crystal templates The organic polymer nanospheres are immersed in the mixed solution until they are thoroughly soaked, and then the excess mixed solution is filtered with a vacuum funnel to obtain a colloidal crystal template, which is then placed in a vacuum oven for low-temperature drying to obtain a dry sample. (3) Colloidal crystal template removal The colloidal crystal template is removed by calcination, and the process is as follows: (A) Pretreatment: Dry the sample at 80-100 ml min -1 The calcination was carried out in a calcination atmosphere at a temperature of 1-3 °C·min -1 The rate is raised from room temperature to 300-350°C, maintained for 4-5h, and then cooled to room temperature; (B) Template removal: The pretreated sample was at 80-100 ml min -1 The calcination was carried out in a calcination atmosphere at a temperature of 1-3 °C·min -1 The temperature was raised from room temperature to 500-550℃ and maintained at 500-550℃ for 5-6h. The catalyst was cooled to obtain a three-dimensional ordered macroporous MnCeTiO x catalyst; (4) Preparation of PTFE calendered membrane The polytetrafluoroethylene resin and the additive are uniformly mixed in a weight ratio of (2-4): (0.1-1), and after standing at 80-100° C. for 12-24 hours, the material is calendered at 40-80° C. to prepare a PTFE calendered film; (5) Preparation of catalytic filter material A layer of adhesive is applied on the surface of the PTFE calendered film and the catalyst is loaded on the PTFE calendered film in a spraying manner, and the catalytic filter material is prepared through the steps of stretching, slitting, curling and needle punching.

2. The method for preparing a three-dimensional ordered macroporous catalytic filter material according to claim 1, characterized in that: In step (1), the complexing agent is one or more of oxalic acid and citric acid.

3. The method for preparing a three-dimensional ordered macroporous catalytic filter material according to claim 1, characterized in that: In step (1), the precursor solution contains a manganese species, a cerium species and titanium dioxide, the manganese species is one of manganese nitrate, manganese chloride or manganese acetate, and the cerium species is one of cerium nitrate, cerium sulfate or cerium acetate.

4. The method for preparing a three-dimensional ordered macroporous catalytic filter material according to claim 3, characterized in that: The precursor solution is a mixed solution of cerium nitrate, manganese nitrate and titanium dioxide, and the mass ratio thereof is (1-4): (1-4): (20-30).

5. The method for preparing a three-dimensional ordered macroporous catalytic filter material according to claim 1, characterized in that: The organic polymer nanospheres in step (2) are one of polystyrene, polymethyl methacrylate and porous silicon microspheres.

6. The method for preparing a three-dimensional ordered macroporous catalytic filter material according to claim 1, characterized in that: The calcination atmosphere in step (3) is nitrogen or air.

7. The method for preparing a three-dimensional ordered macroporous catalytic filter material according to claim 1, characterized in that: The auxiliary agent in step (4) is one of kerosene, liquid paraffin and petroleum ether.

8. The method for preparing a three-dimensional ordered macroporous catalytic filter material according to claim 1, characterized in that: The binder in step (5) is one of coal tar, organic titanium coupling agent or epoxy resin adhesive.

9. A three-dimensional ordered macroporous catalytic filter material prepared by the method according to any one of claims 1 to 8.

10. Use of the three-dimensional ordered macroporous catalytic filter material according to claim 9 in preparing a product for removing organic matter and particulate matter from water.

Citation Information

Patent Citations

  • Three-dimensional ordered macroporous oxide catalyst for diesel soot purification and preparation method thereof

    CN101733110A

  • Preparation and application of perovskite catalyst with three-dimensional ordered macroporous structure

    CN104399480A

  • Ordered mesoporous structure manganese cerium titanium catalyst as well as preparation method and application thereof

    CN106984301A

  • Vacuum ultraviolet photocatalytic purification material as well as preparation method and application thereof

    CN109046326A

  • Three-dimensional ordered macroporous structure (3DOM)-manganese cerium titanium composite oxide denitration catalyst and preparation method thereof

    CN113198460A

Cited By

  • Preparation method and application of PTFE catalytic filter material

    CN119657231A

  • Preparation method and application of PTFE catalytic filter material

    CN119657231B