Forging method of nickel-based alloy forge piece for nuclear power
Through the secondary smelting and four upsetting and three-extraction forging processes of vacuum induction furnace + electroslag remelting furnace, combined with solid solution heat treatment and quality control, the problems that are difficult to meet the complexity and performance requirements of NS3105 alloy forging process are solved, and nickel-based alloy forging is realized The high purity and excellent mechanical properties reduce the risk of stress corrosion fracture.
Patent Information
- Application Number
- CN202411131285.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-17
- Publication Date
- 2024-11-22
AI Technical Summary
The forging process of NS3105 alloy is complex, with strict chemical composition and performance requirements. It is difficult for the existing technology to effectively control the heating temperature, forging deformation and cooling speed, which makes it difficult for the forging performance and tissue structure to meet the requirements, especially in terms of stress corrosion and rupture.
The NS3105 electroslag ingot is manufactured by secondary smelting of vacuum induction furnace + electroslag remelting furnace, precisely control chemical composition, adopt the forging process of four upsets and three pulls, design solid-solution heat treatment and supplementary heat treatment processes, and combine with a strict quality control system to ensure forgings High purity and excellent mechanical properties.
By precisely controlling chemical composition and process parameters, the purity and mechanical properties of nickel-based alloy forgings are significantly improved, meeting the high requirements in the field of nuclear power, reducing the risks of forging defects and stress corrosion and fracture, and improving the pass rate and reliability of the product.
Smart Images

Figure CN118989203A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of alloy forging, and in particular to a forging method of nickel-based alloy forgings for nuclear power. Background Art
[0002] Nuclear power forgings mainly refer to high-temperature alloys for reactors. These alloys are mainly used as steam generator heat transfer tubes, component frames and compression springs, as well as superheater and reheater heat transfer tube components for high-temperature gas-cooled reactors and some fast reactors.
[0003] In pressurized water reactor (PWR) nuclear power plants, the most critical material is the high-temperature alloy used in the heat transfer tubes of the steam generator. The evaporator is a key device for heat exchange between the primary and secondary circuits in a PWR nuclear power plant. The service conditions of its heat transfer tubes are harsh. There is not only the pressure difference between the primary and secondary working media inside and outside the tube, but also a comprehensive corrosion in the high-temperature water medium, including uniform corrosion, pitting corrosion, crevice corrosion, intergranular corrosion, and stress corrosion cracking (SCC). Among them, stress corrosion cracking is the most common form of evaporator heat transfer tube failure. Many reactors have experienced this problem. Damage to the evaporator heat transfer tube can affect the normal operation of the reactor, resulting in forced power reduction or even shutdown accidents, resulting in huge economic losses and potentially threatening the safe operation of the nuclear power plant.
[0004] NS3105, also known as lnconel690 alloy, is an austenitic high-chromium nickel-based corrosion-resistant alloy. With its excellent corrosion resistance and high strength, it has gradually become an ideal material for nuclear power steam generator pipes. It not only has better resistance to stress corrosion cracking than 304 stainless steel, Incoloy800 alloy, and In-conel600 alloy in chloride-containing solutions and sodium hydroxide solutions, but also shows a low corrosion rate and excellent stress corrosion cracking resistance, especially in various types of high-temperature water. Therefore, it is widely used in nuclear power steam units.
[0005] However, the forging process of NS3105 alloy is complex, with strict requirements on chemical composition and performance, and high requirements on purity and stability. It requires precise control of parameters such as heating temperature, forging deformation, and cooling rate to ensure that the performance and organizational structure of the alloy meet the requirements. Summary of the Invention
[0006] The purpose of this application is to provide a forging method for forging nickel-based alloy forgings for nuclear power using NS3105 alloy steel, which can obtain nickel-based alloy forgings with higher purity and excellent mechanical properties to meet higher usage indicators.
[0007] The present application provides a forging method for a nickel-based alloy forging for nuclear power, which adopts the following technical solution: A forging method for nickel-based alloy forgings for nuclear power, comprising the following steps: a. NS3105 electroslag steel ingots are manufactured by secondary smelting in a vacuum induction furnace + electroslag remelting furnace, wherein the chemical composition is controlled in the following mass percentages: C: 0.010-0.040%; Si: ≤0.50%; Mn: ≤0.50%; P: ≤0.015%; S: ≤0.008%; Ni: ≥58.0%; Cr: 28.0-31.0%; Fe: 8.0-11.0%; Cu: ≤0.10%; Co: ≤0.080%; Ti: ≤0.30%; Al: ≤0.20%; B ≤0.0005%; During the smelting process of the steel ingot, the mass percentage content of C is controlled to be 0.020-0.040%, the mass percentage content of Mn is 0.20-0.50%, the mass percentage content of Cr is 29.50-31.00%, the mass percentage content of Ti is 0.15-0.30%, and the mass percentage content of Al+Ti is limited to 0.45-0.50%; b. Heating of electroslag steel ingots: heating in the furnace with an initial temperature of less than or equal to 600°C, heating to 850±20°C at a heating rate of ≥80°C / h for 4 hours, holding the temperature for 1.5 hours, then heating the temperature to 1160±20°C for 1.5 hours, holding the temperature for 2 hours, and then forging; c. Forging deformation of forgings, using a four-upsetting and three-drawing forging process, with a total forging ratio greater than 8, to obtain rough forgings of nickel-based alloy forgings; d. First rough machining, machining the rough forging to the required first rough size; e. Solution heat treatment: put into the furnace at ≤400℃ and heat to 1020±10℃ and keep it for 3.5-4h, then water cool to ≤70℃; Supplementary heat treatment: heat up to 715±10℃ with the furnace and keep it for 7-7.5h, then air cool and control the grain size to ≥5 level; f. Sampling: take samples from the heat-treated rough forgings according to the sampling diagram; g. Physical and chemical performance testing; h. Final machining, forgings are processed to the required final delivery drawing dimensions; i. Non-destructive testing; j. Appearance and dimension inspection; k. Label the finished product.
[0008] By adopting the above technical solutions: precise control of chemical composition, optimization of smelting and heat treatment processes, strict forging and processing procedures, and comprehensive quality control, nickel-based alloy forgings for nuclear power with high purity and excellent mechanical properties can be obtained, meeting the high requirements for materials in the nuclear power field.
[0009] Analyzing the reasons, the possible reasons are: 1) The NS3105 electroslag steel ingot is manufactured by the method of secondary melting in a vacuum induction furnace and an electroslag remelting furnace. This combined melting method can significantly reduce the impurity content in the steel ingot, including gases (such as H, O, N), non-metallic inclusions and harmful elements (such as S, P, etc.). The initial melting in the vacuum induction furnace helps to remove most impurities, while the electroslag remelting further refines the steel ingot to ensure the high purity of the steel ingot. 2) Precisely control the mass percentage of each chemical component in the steel ingot, especially the content of key elements such as C, Mn, Cr, Ti, and Al. These elements have a significant impact on the mechanical properties of the alloy. For example, the C and Cr content affects the hardness and corrosion resistance of the alloy, while the Mn and Ti content is related to the strength and toughness of the alloy. By finely controlling these elements, nickel-based alloy forgings with excellent mechanical properties can be obtained; 3) The designed solution heat treatment and supplementary heat treatment processes are intended to optimize the alloy's microstructure, improve grain uniformity and refinement, and thus enhance the alloy's strength and toughness. The solution heat treatment redissolves the precipitated phases in the alloy into the matrix. The subsequent supplementary heat treatment controls grain growth and ensures a grain size of ≥5, which is crucial for improving the alloy's long-term strength, creep resistance, and fatigue resistance. 4) The forging process of four upsetting and three drawing is adopted, with a total forging ratio greater than 8, which ensures the density and uniformity of the internal structure of the forging and reduces forging defects. At the same time, through multiple rough processing and final machining, the forging size is ensured to be accurate and meet the design requirements; 5) Sampling, physical and chemical performance testing, non-destructive testing, appearance and dimensional inspection and other links ensure that the quality of forgings meets the standards and design requirements. The comprehensive quality control system helps to detect and correct problems in a timely manner and improve the qualification rate and reliability of products.
[0010] Preferably, the chemical components of the NS3105 electroslag steel ingot are controlled within the following mass percentages: C: 0.020-0.040%; Si: ≤0.50%; Mn: 0.20-0.50%; P: ≤0.015%; S: ≤0.008%; Ni: ≥58.0%; Cr: 29.5-31.0%; Fe: 8.0-11.0%; Cu: ≤0.10%; Co≤0.080%; Ti: 0.15-0.30%; Al: ≤0.20%; B≤0.0005%; As≤0.01%; Sn≤0.01%; Sb≤0.002%; Pb≤0.001%; H≤0.0004%; O≤0.002%; N≤0.004%.
[0011] By adopting the above technical solutions: Preferably, the Ti / C weight percentage of the NS3105 electroslag steel ingot is controlled to be 7.
[0012] By adopting the above technical solution: the formation and distribution of carbides can be optimized, the forging and heat treatment processes can be stabilized, the appropriate amount of carbides can improve the hardness and wear resistance of the alloy, help to obtain ideal mechanical properties and processing properties, and can reduce the formation of hot cracks and cold cracks, obtain a more uniform organizational structure, improve the toughness and crack resistance of the alloy, and improve the process stability.
[0013] Preferably, the dimensions of the nickel-based alloy forging are an outer diameter of Φ430 mm and a height of 135 mm.
[0014] By adopting the above technical solution: the dimensions designed according to specific application scenarios and performance requirements can ensure the rational use of materials and avoid waste. At the same time, the dimensions may also take into account the material fluidity and deformation characteristics during the forging process, which helps to reduce forging defects and improve product quality.
[0015] Preferably, the forging deformation includes the following steps in sequence: blanking heating, four times of upsetting, three times of drawing, gradual forming according to process dimensions, and cooling after forging.
[0016] By adopting the above technical solution: the forging deformation process is refined to make each operation more precise and controllable. The alternating four upsetting and three drawing steps helps to improve the internal structure of the material, eliminate internal defects such as pores and looseness, and promote material densification. At the same time, it can also make the material deform more evenly during the forging process, reducing stress concentration and cracking. The gradual shaping process according to the process size ensures the accuracy and consistency of the final size of the forging. The deformation amount of each step is precisely controlled to reduce the material cracks or dimensional deviation caused by excessive deformation, thereby improving the overall quality of the forging. The steps of blanking heating and post-forging cooling are crucial for controlling the temperature during the forging process. Appropriate heating temperature helps reduce the deformation resistance of the material, improve the plasticity and forgeability of the material, making it easier to achieve the required deformation, while post-forging cooling helps stabilize the material's organizational structure and prevent grain growth and performance degradation due to overheating.
[0017] In summary, this application includes at least one of the following beneficial technical effects: 1. This application uses a secondary melting process of a vacuum induction furnace + an electroslag remelting furnace to effectively remove impurities in the steel ingot, such as gas, non-metallic inclusions, and harmful elements, significantly improving the purity of the steel ingot. At the same time, the chemical composition, especially the content of key elements such as C, Cr, and Ti, is precisely controlled to optimize the microstructure of the alloy. The resulting nickel-based alloy forgings have excellent mechanical properties and high purity, meeting the high material requirements of the nuclear power industry. 2. The forging deformation process in this application is refined into multiple steps, including blanking heating, four upsetting steps, three stretching steps, gradual shaping according to process dimensions, and post-forging cooling. This refined operation makes each step more precise and controllable. The alternating upsetting and stretching steps improve the internal structure of the material, eliminate internal defects, promote material densification, and reduce stress concentration and cracking. In addition, the optimization of the solution heat treatment and supplementary heat treatment processes further stabilizes the material's structure, refines the grain size, and improves the alloy's long-term strength and creep resistance. 3. The entire forging process of this application, from the preparation, smelting, forging, heat treatment of raw materials to final processing, inspection and labeling, follows strict quality control standards. Through strict control of multiple links such as sampling, physical and chemical property testing, non-destructive testing, and appearance and dimensional inspection, the quality of the forgings is ensured to meet the design requirements. The standardized production process improves production efficiency and product consistency, reduces production costs, and makes this method have broad application prospects and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 Schematic diagram of the heating process of S3105 nickel-based alloy steel in an embodiment of the present application; Figure 2 This is a schematic diagram of the dimensions of a forging subjected to the first rough machining in an embodiment of the present application; Figure 3 This is a schematic diagram of the performance heat treatment process of nickel-based alloy forgings for nuclear power use in an embodiment of the present application; Figure 4 This is a schematic diagram of the sampling position of the forgings in the embodiment of the present application; Figure 5 This is a schematic diagram of the appearance and dimensions of a forging according to an embodiment of the present application; Figure 6 2. It is a schematic diagram of the non-metallic inclusion detection results of the forgings according to the embodiment of the present application; Figure 7 2. It is a schematic diagram of the grain size test results of the forgings according to the embodiment of the present application; Figure 8 It is a flow chart of the forging deformation steps of the forging in the embodiment of the present application. DETAILED DESCRIPTION
[0019] The present invention is further described below with reference to embodiments. The embodiments and drawings are only used for explanation and are not used to limit the scope of protection of the present invention.
[0020] Nickel-based alloy forgings for nuclear power are widely used in nuclear reactor equipment due to their excellent high temperature resistance, corrosion resistance and mechanical properties. In this embodiment, NS3105 steel is used to manufacture nickel-based alloy forgings for nuclear power.
[0021] Nickel-based alloy forgings for nuclear power use NS3105 steel to manufacture specific dimensions of forgings with an outer diameter of Φ430mm and a height of 135mm. Its various indicators must meet and satisfy the technical conditions specified below, specifically including the smelting, heating, forging, performance heat treatment, physical and chemical property testing, and final processing of NS3105 steel.
[0022] The goal is to ensure that the manufactured forgings meet and achieve all technical indicators in the technical conditions of nickel-based alloy forgings for nuclear power and complete the requirements for localization.
[0023] (1) Technical indicators of the technical conditions for the development of nickel-based alloy forgings for nuclear power using NS3105 nickel-based alloy steel: ① Table 1: Chemical composition of NS3105 nickel-based alloy steel (%) ② Table 2: Mechanical properties ③ Table 3: Non-metallic inclusions ④ Grain size: The grain size of forgings should be equal to or finer than grade 5.
[0024] ⑤Intergranular corrosion: After immersion in boiling solution for 24 hours, there is no tendency of intergranular corrosion.
[0025] ⑥ Non-destructive visual inspection: according to NB / T20003.7 standard; Liquid penetrant test: according to NB / T20003.4 standard; Ultrasonic inspection: according to the quality grade standard of Class I in Table 14 of NB / T20003.2.
[0026] (2) Process route: smelting of electroslag steel ingots (MIV+ESR) and blanking of round steel → blanking → heating of blanks → forging of blanks → rough machining (Ⅰ) → solution heat treatment + supplementary heat treatment → sampling → physical and chemical testing → final machining (Ⅱ) → non-destructive testing (VT, PT, UT) → appearance and dimension inspection → packaging and issuance of quality certificate after passing the test. Example
[0027] A forging method for a nickel-based alloy forging for nuclear power, comprising the following steps: a. Electrode rods manufactured using a vacuum induction furnace + electroslag remelting furnace secondary smelting to produce NS3105 (690) electroslag ingots, Ti / C weight percentage is controlled to 7, the content of each component refer to Table 1; b. Figure 1As shown, the heating of electroslag steel ingot from blanking to round steel is carried out by heating in the furnace at an initial temperature of 600°C, heating to 860°C at a heating rate of 90°C / h for 4 hours, holding at that temperature for 1.5 hours, heating to 1160°C for 1.5 hours, and holding at that temperature for 2 hours before forging; c. Forging deformation of the forging, using a four-upsetting and three-drawing forging process, with a forging ratio greater than 8, to obtain a rough forging. In this embodiment, the forging deformation is carried out in the following steps, such as Figure 8 As shown; i. Cutting and heating: 3 tons of electroslag steel ingots are used to cut into φ235 round steel batches. The material utilization rate is 90%, that is, 120kg of the ingot head and 180kg of the ingot tail should be removed. Cutting on the sawing machine: size: φ235×371 / piece. Heating is carried out according to the heating specifications, and on-site records are kept; ii. For upsetting, pay attention to flatness, forging ratio r = 1.5, for drawing, forging ratio r = 1.8; iii. Secondary upsetting, pay attention to flatness, forging ratio r = 1.9, drawing, forging ratio r = 1.9; iv. Three times of upsetting, pay attention to flatness, forging ratio r = 2.2, drawing, forging ratio r = 1.9; v. Upset four times, pay attention to flatness, forging ratio r = 3.3, gradually follow the process size, make good on-site records, and gradually make good markings, R 总 =14.5; vi. Post-forging cooling step, using air cooling; vii. Inspection.
[0028] d. First rough machining, forging dimensions refer to Figure 2 , rough machining the forging to Figure 2 Size, the weight of the forging is 141Kg; e. Figure 3 As shown, solution heat treatment, heat treatment of 1 batch, each batch of 4 forgings as test pieces, put into the furnace at 300 ℃ and heat up to 1020 ℃, keep warm for 3.5 hours, and water cool to 65 ℃; supplementary heat treatment, heat up to 715 ℃ and keep warm for 7 hours and air cool, control the grain size at level 5; f. Sampling, sampling according to the sampling map position see Figure 4 ; g. Physical and chemical performance testing; h. Final machining, final delivery dimensions of forgings are as follows Figure 5 As shown; i. Ultrasonic UT non-destructive testing; The testing work is carried out according to the established process route, and its chemical composition is tested according to GB / T223; Mechanical properties testing: room temperature tensile test according to GB / T228.1-2010; high temperature tensile test according to GB / T228.2-2015; Brinell hardness test according to GB / T231.1-2018; Conduct non-metallic inclusion detection tests according to GB / T10561-2005; Carry out grain size test according to GB / T6394-2017; The test results are as follows: like Figure 3 As shown, the number of sampling (tangential sampling) is as follows: Room temperature tensile specimens, corresponding to serial numbers 1 and 8; 350℃ tensile specimens, corresponding to serial numbers 2 and 9; Room temperature impact specimens, corresponding to serial numbers 3, 4, and 5; Intergranular corrosion specimens, corresponding to serial numbers 10 and 11; Hardness specimen, corresponding to serial number 6; Metallographic specimen, corresponding to serial number 12; Finished product analysis sample, corresponding to serial number 13.
[0029] As can be seen from the above table, the measured values are all within the optimized composition range, especially the precise control of the contents of key elements such as C, Cr, and Ni, which lays the foundation for achieving excellent performance. The tensile test results show that the tensile strength, yield strength, elongation and other performance indicators of the forgings at room temperature and high temperature are all better than the standard requirements, indicating excellent mechanical properties. The hardness test and grain size detection test results show that the hardness and grain size of the forgings are well controlled, meeting the high requirements of nuclear power materials.
[0030] This may be because the secondary melting method of vacuum induction furnace + electroslag remelting furnace can significantly reduce the impurity content in the steel ingot, including gases (such as H, O, N) and non-metallic inclusions and harmful elements (such as As, Sn, Sb, Pb, etc.). High-purity steel ingots are the basis for manufacturing high-quality nickel-based alloy forgings. Initial melting in a vacuum induction furnace removes most impurities, followed by further refining with electroslag remelting. This combination ensures high purity and uniformity of the ingot. The C and Cr contents affect the hardness and corrosion resistance of the alloy, while the Mn and Ti contents are related to the strength and toughness of the alloy. Controlling the Ti / C weight ratio at 7 helps ensure the formation of an appropriate amount of carbides in the alloy, neither too much nor too little. Excessive carbides may make the alloy brittle, while too little carbides may not fully exert the effect of dispersion strengthening, ultimately resulting in a nickel-based alloy with excellent mechanical properties and corrosion resistance. In addition, entering the furnace at an initial temperature of less than or equal to 600°C and controlling the heating rate can effectively avoid excessive thermal stress in the steel ingot during the heating process, reduce defects such as cracking, and ensure uniform temperature distribution inside the steel ingot, providing suitable temperature conditions for subsequent forging. At the same time, the forging process of four upsetting and three drawing is adopted, and the total forging ratio is greater than 8, which can ensure the density and uniformity of the internal structure of the forging and reduce forging defects such as holes and cracks. During the forging process, the material undergoes plastic deformation, the grain is refined, and the structure is more uniform, thereby improving the mechanical properties and processing performance of the forging; The heat treatment process (solution heat treatment and supplementary heat treatment) can adjust the distribution of the precipitated phase of the alloy, improve the alloy's long-term strength, creep resistance and fatigue resistance, accurately control the heat treatment temperature and holding time, ensure that the precipitated phase in the alloy is redissolved into the matrix, and control the grain growth to obtain an ideal microstructure.
[0031] During the heat treatment process, the choice of water cooling or air cooling (air cooling) plays a crucial role in controlling the phase transformation kinetics and grain size of the alloy. Considering that excessive grain size growth will significantly weaken the toughness of the workpiece, a reasonable cooling strategy becomes particularly important.
[0032] The water cooling method, with its efficient heat transfer capability, can rapidly cool the alloy from a high temperature state to a lower temperature in a very short time. This rapid cooling rate effectively inhibits the precipitation process of the precipitated phase and significantly reduces the growth trend of the grains, thereby achieving the refinement of the alloy microstructure. The refined microstructure helps to improve the mechanical properties of the alloy, including strength, hardness, and possible toughness (although rapid cooling may affect toughness in some cases, grain refinement itself usually has a positive effect on toughness).
[0033] In contrast, air cooling provides a relatively mild cooling environment, allowing the alloy to gradually cool to room temperature at a slower cooling rate. This cooling method may allow some precipitated phases to precipitate over a longer period of time and result in a certain degree of grain growth. Moderate grain growth may be beneficial in some cases because it can balance the strength and toughness of the alloy, especially in application scenarios that require a certain degree of toughness.
[0034] In the heat treatment process of the present application, water cooling is first used to quickly suppress phase transformation and grain growth, and then switched to air cooling to achieve more uniform cooling and possible precipitation phase control. This combined water cooling and air cooling strategy can fully utilize the advantages of the two cooling methods to obtain an alloy material with ideal microstructure and properties.
[0035] The above are all modifications that a person skilled in the art can make to this embodiment as needed after reading this specification, which do not contribute creatively or solutions that obviously constitute technical inspiration. However, as long as they are within the scope of the claims of this application, they should be protected by patent law.
Claims
1. A forging method for a nickel-based alloy forging for nuclear power, characterized in that: The steps include: a. NS3105 electroslag steel ingot is manufactured by secondary smelting in vacuum induction furnace + electroslag remelting furnace, wherein each chemical composition is controlled within the following mass percentages: C: 0.010-0.040%; Si: ≤ 0.50%; Mn: ≤ 0.50%; P: ≤ 0.015%; S: ≤ 0.008%; Ni: ≥ 58.0%; Cr:
28. 0-31.0%; Fe: 8.0-11.0%; Cu: ≤ 0.10%; Co: ≤ 0.080%; Ti: ≤ 0.30%; Al: ≤ 0.20%; B ≤ 0.0005%; During the smelting process of ingot steel, the mass percentage content of C is controlled to be 0.020-0.040%, the mass percentage content of Mn is controlled to be 0.20-0.50%, the mass percentage content of Cr is controlled to be 29.50-31.00%, the mass percentage content of Ti is controlled to be 0.15-0.30%, and the mass percentage content of Al+Ti is controlled to be limited to 0.45-0.50%; b. Heating of electroslag ingots: heating in the furnace at an initial temperature of 600°C or less, heating to 850±20°C at a heating rate of 80°C / h or more for 4h, keeping the temperature for 1.5h, heating to 1160±20°C for 1.5h, keeping the temperature for 2h, and then forging; c. Forging deformation of forgings, using a four-upsetting and three-drawing forging process for forging, with a total forging ratio greater than 8, to obtain a rough forging of a nickel-based alloy forging; d. The first rough machining is to process the rough forging to the required first rough size; e.Performance heat treatment; f. Sampling: take samples from the rough forgings after heat treatment according to the sampling map; g. Physical and chemical properties test; h. Final machining, forgings are processed to the required final delivery drawing dimensions; i. Non-destructive testing; j. Appearance and dimension inspection; k. Label the finished product.
2. The forging method of nickel-based alloy forgings for nuclear power according to claim 1, characterized in that: The chemical components of the NS3105 electroslag steel ingot are controlled within the following mass percentages: C: 0.020-0.040%; Si: ≤ 0.50%; Mn: 0.20-0.50%; P: ≤ 0.015%; S: ≤ 0.008%; Ni: ≥ 58.0%; Cr: 29.5-31.0%; Fe: 8.0-11.0%; Cu: ≤ 0.10%; Co ≤0.080%; Ti:0.15-0.30%; Al: ≤0.20%; B≤0.0005%; As≤0.01%; Sn≤0.01%; Sb≤0.002%; Pb≤0.001%; H≤0.0004%; O≤0.002%; N≤0.004%.
3. The forging method of nickel-based alloy forgings for nuclear power according to claim 1, characterized in that: The Ti / C weight percentage of the NS3105 electroslag steel ingot is controlled to be 7.
4. The forging method of nickel-based alloy forgings for nuclear power according to claim 1, characterized in that: The dimensions of the nickel-based alloy forging are an outer diameter of Φ430 mm and a height of 135 mm.
5. The forging method of nickel-based alloy forgings for nuclear power according to claim 1, characterized in that: The forging deformation in step c includes: heating of blanking, four times of upsetting, three times of drawing, gradual forming according to process dimensions, and cooling after forging.
6. The forging method of nickel-based alloy forgings for nuclear power according to claim 1, characterized in that: The performance heat treatment in step e includes solution heat treatment and supplementary heat treatment.
7. The forging method of nickel-based alloy forgings for nuclear power according to claim 6, characterized in that: The solution heat treatment is specifically as follows: entering the furnace at ≤400°C, heating with the furnace to 1020±10°C, and keeping the temperature for 3.5-4h, and then water cooling to ≤70°C.
8. The forging method of nickel-based alloy forgings for nuclear power according to claim 6, characterized in that: The supplementary heat treatment is specifically as follows: heating the furnace to 715±10°C and keeping the temperature for 7-7.5h, air cooling, and controlling the grain size to be ≥5.
Citation Information
Patent Citations
Heat treatment method of large-size, high-strength and fine-grain nickel-based superalloy forge piece for nuclear reactor
CN104674144A
Method for manufacturing large high-purity nickel base alloy forging
CN104988356A
Forging method for flange forge piece of nuclear power steam generator
CN107760990A
Nickel-based alloy large-section bar used for nuclear power critical equipment and manufacturing method of large-section bar
CN109136652A
Technological method of reducing number of metallurgical defects of GH4169 nickel base alloy ingot
CN110484775A