Preparation method and system of LPBF magnesium alloy tissue engineering scaffold with smooth inner surface

By optimizing the contour scanning strategy and spot compensation value of LPBF magnesium alloy tissue engineering scaffolds, the defects of powder adhesion and slag adhesion were solved, the flowability and corrosion resistance of the scaffolds were improved, a smooth inner surface and high density were achieved, and the production process was simplified.

CN118989355APending Publication Date: 2024-11-22SHANGHAI JIAOTONG UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411071907.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the existing technology, LPBF magnesium alloy tissue engineering scaffolds are prone to powder adhesion and slag buildup defects during the preparation process, resulting in poor flowability, decreased fatigue and corrosion performance of porous scaffolds, and difficulty in achieving a smooth inner surface, which affects the mechanical strength and biocompatibility of the scaffolds.

Method used

By optimizing the contour scanning strategy and spot compensation value, using single-pass contour scanning and filling scanning, and combining the contour scanning before and after and the filling compensation value, the laser power and scanning speed are adjusted to eliminate powder adhesion and slag defects, thereby improving the density and surface smoothness of the scaffold.

Benefits of technology

This technology achieves a smooth inner surface for porous supports, improving flowability and corrosion resistance, simplifying post-processing, reducing production costs, and expanding the printable size and structural design freedom of supports.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989355A_ABST
    Figure CN118989355A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and system of an LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface, and the preparation method comprises the following steps: S1, scanning a porous scaffold, and screening out the most compact filling scanning parameters; the scanning comprises single-pass contour scanning and single-pass filling scanning; s2, optimizing a contour scanning strategy according to the most compact filling scanning parameter; s3, obtaining a corresponding molten pool size, and adjusting a light spot compensation value by using an optimized contour scanning strategy; and S4, preparing the magnesium alloy tissue engineering scaffold based on a contour scanning strategy and the adjusted light spot compensation value. According to the method, the powder sticking and slag adhering defects which seriously influence the inner surface roughness and the stent performance in the complex porous structure can be eliminated in situ in the preparation process, the liquidity, fatigue and corrosion resistance of the porous stent are improved, the tedious aftertreatment process is simplified, the production cost is reduced, and the concept of green production is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of biomedical material preparation, and in particular to a method and system for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface. Background Art

[0002] 1. Large bone defects caused by trauma, disease, developmental malformation, revision surgery, tumor resection or osteomyelitis, with a defect length exceeding 2-2.5 times the diameter of the defect bone, are one of the major challenges in orthopedic clinical treatment. An ideal bone scaffold must have sufficient mechanical strength, corrosion resistance and biocompatibility to meet its load-bearing function; at the same time, the scaffold should have an interconnected porous network to deliver nutrients and allow cell migration. Among many additive manufacturing technologies, laser powder bed melting (LPBF) technology has the advantages of high structural design freedom, high preparation accuracy, short development cycle, and avoidance of subsequent mechanical processing. Therefore, it is widely used in the preparation of bone tissue engineering scaffolds. Compared with autologous or allogeneic bone transplant scaffolds, LPBF magnesium alloy tissue engineering scaffolds have the advantages of being artificially manufactured, low-cost, and no immune rejection reaction; compared with polymer scaffolds, it has the advantages of good biocompatibility, osteogenicity, and high mechanical strength, and has received widespread attention in recent years. However, magnesium alloy has a low boiling point and high vapor pressure, which will cause serious powder evaporation and splashing during the 3D printing process. At the same time, due to the low melting point, high thermal conductivity and low surface tension of magnesium, it is easy to produce a large molten pool and heat-affected zone. A large amount of unmelted powder is very likely to adhere to the surface and inside of the porous bracket, forming a powder sticking defect. Under the horizontal overhanging structure inside the bracket, after the laser melts the powder, the melt infiltrates into the powder below under the action of gravity and capillary force, causing a large amount of powder to adhere to the lower surface of the overhanging structure to form a slag defect. The formation process of slag defects is as follows: Figure 2 shown.

[0003] 2. Powder and slag inside the stent will reduce the fluidity, fatigue and corrosion resistance of the porous stent. When the pore size of the stent is small, the powder on the inner surface will hinder the entry of the external polishing medium, and the fluidity will become worse the further into the stent. The larger the size of the stent, the more difficult it is to polish the inner surface. In severe cases, the detached powder particles will mechanically interlock with the originally adhered powder, causing the internal pores to be completely blocked and the three-dimensional connectivity of the stent to be lost. In addition, after the porous stent is implanted in the human body, it needs to withstand periodic loads. Powder adhesion causes the surface roughness of the stent to increase significantly. On the one hand, it promotes the initiation of surface fatigue cracks, and on the other hand, it increases the contact area between the stent and the corrosive medium, which will greatly accelerate the corrosion of the stent and produce a large amount of hydrogen, which will then form emphysema at the implantation site.

[0004] 3. In order to improve the surface smoothness, porous stents often use post-processing processes such as chemical or electrochemical polishing. Since magnesium alloys will produce a large amount of hydrogen in the acidic polishing liquid, the polishing liquid will seriously inhibit the flow of the polishing liquid into the interior of the stent, resulting in the exterior of the stent being easier to polish to the target rod diameter, but the interior being difficult to polish to the target rod diameter, ultimately resulting in thinner struts at the edge of the stent and thicker struts inside. The larger the stent size, the smaller the pore size, and the worse the permeability of the structure (the ease with which the fluid flows in the porous medium), the more obvious the difference in rod diameters inside and outside. Therefore, for LPBF magnesium alloy porous stents, there is an urgent need for a molding method that can effectively reduce the defects of powder sticking and slag hanging inside the stent, and improve the corrosion resistance and corrosion fatigue performance of the magnesium alloy porous stent. Summary of the invention

[0005] In view of the defects in the prior art, the object of the present invention is to provide a method and system for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface.

[0006] According to the present invention, a method for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface comprises:

[0007] Step S1: Scan the porous scaffold to select the most dense filling scanning parameters;

[0008] The scanning includes a single-pass contour scan and a single-pass fill scan;

[0009] Step S2: Optimizing the contour scanning strategy according to the most dense filling scanning parameters;

[0010] Step S3: Obtain the corresponding molten pool size and adjust the spot compensation value using the optimized contour scanning strategy;

[0011] Step S4: preparing a magnesium alloy tissue engineering scaffold based on the contour scanning strategy and the adjusted spot compensation value.

[0012] Preferably, the step S1 comprises:

[0013] The porous scaffold was subjected to a single contour scan and a single filling scan. The contour scan parameters were consistent with the filling scan parameters. After preparation, the sample was cut parallel to the preparation direction. The cross section was polished to obtain its optical microscopic image and analyze its density. Among the parameter combinations with a density greater than 99.5%, the parameter with 0.05≤P / V≤0.5 was selected and set as P 填 、V 填 ;

[0014] Where P is the laser power and V is the scanning speed.

[0015] Preferably, the step S2 comprises:

[0016] Select fill scan parameter as P填 、V 填 , let the contour scanning parameter be P 轮 、V 轮 , the number of contour scans is PT, and the contour parameters are calculated:

[0017]

[0018] Among them, the contour line energy density scaling factor Z=5~30, within the range of the contour compensation value, the contour pre-scan and contour post-scan can be scanned multiple times, and the scanning sequence includes from the inner circle contour scanning to the outer circle contour scanning, or from the outer circle contour scanning to the inner circle contour scanning; the contour pre-scan and contour post-scan can select different laser powers P, scanning speeds V, contour scanning times PT, contour line energy density scaling factors Z and contour compensation values ​​PC; the setting range of the filling compensation value FC is 0≤FC≤PC.

[0019] Preferably, step S3 comprises:

[0020] Obtain the molten pool width under the structure and process parameters, and optimize the spot compensation value;

[0021] Assume that the wall thickness / rod diameter of the original design stent model is T0, and the wall thickness / rod diameter after the optimized contour scanning strategy is T1, then the spot compensation value is:

[0022]

[0023] Where SZ is the spot diameter, R 熔 For the corresponding P 填 / V 填 The size increase caused by multiple contour scans is compensated by adjusting the spot compensation value.

[0024] Preferably, step S1 further includes setting multiple pre-contour scans with a certain energy density according to the specific stent structure and the length of the lower surface overhang area before the filling scan; and setting multiple post-contour scans with a certain energy density according to the surface powder adhesion of the specific stent after the filling scan.

[0025] According to the present invention, a system for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface is provided, comprising:

[0026] Module M1: Scan the porous scaffold and select the most dense filling scanning parameters;

[0027] The scanning includes a single-pass contour scan and a single-pass fill scan;

[0028] Module M2: Optimize the contour scanning strategy based on the most dense filling scanning parameters;

[0029] Module M3: Obtain the corresponding molten pool size and adjust the spot compensation value using the optimized contour scanning strategy;

[0030] Module M4: Preparation of magnesium alloy tissue engineering scaffolds based on contour scanning strategy and adjusted spot compensation value.

[0031] Preferably, the module M1 comprises:

[0032] The porous scaffold was subjected to a single contour scan and a single filling scan. The contour scan parameters were consistent with the filling scan parameters. After preparation, the sample was cut parallel to the preparation direction. The cross section was polished to obtain its optical microscopic image and analyze its density. Among the parameter combinations with a density greater than 99.5%, the parameter with 0.05≤P / V≤0.5 was selected and set as P 填 、V 填 ;

[0033] Where P is the laser power and V is the scanning speed.

[0034] Preferably, the module M2 comprises:

[0035] Select fill scan parameter as P 填 、V 填 , let the contour scanning parameter be P 轮 、V 轮 , the number of contour scans is PT, and the contour parameters are calculated:

[0036]

[0037] Among them, the contour line energy density scaling factor Z=5~30, within the range of the contour compensation value, the contour pre-scan and contour post-scan can be scanned multiple times, and the scanning sequence includes from the inner circle contour scanning to the outer circle contour scanning, or from the outer circle contour scanning to the inner circle contour scanning; the contour pre-scan and contour post-scan can select different laser powers P, scanning speeds V, contour scanning times PT, contour line energy density scaling factors Z and contour compensation values ​​PC; the setting range of the filling compensation value FC is 0≤FC≤PC.

[0038] Preferably, the module M3 includes:

[0039] Obtain the molten pool width under the structure and process parameters, and optimize the spot compensation value;

[0040] Assume that the wall thickness / rod diameter of the original design stent model is T0, and the wall thickness / rod diameter after the optimized contour scanning strategy is T1, then the spot compensation value is:

[0041]

[0042] Where SZ is the spot diameter, R 熔 For the corresponding P填 / V 填 The size increase caused by multiple contour scans is compensated by adjusting the spot compensation value.

[0043] Preferably, the module M1 also includes setting multiple pre-contour scans with a certain energy density according to the specific support structure and the length of the lower surface overhang area before the filling scan; and setting multiple post-contour scans with a certain energy density according to the surface powder adhesion of the specific support after the filling scan.

[0044] Compared with the prior art, the present invention has the following beneficial effects:

[0045] 1. The present invention can eliminate the powder sticking and slag defects inside the complex porous structure that seriously affect the inner surface roughness and the performance of the bracket in situ during the preparation process, improve the fluidity, fatigue and corrosion resistance of the porous bracket, simplify the cumbersome post-processing process, reduce the production cost, and realize the concept of green production.

[0046] 2. The present invention greatly broadens the maximum printable size of the porous scaffold, reduces the minimum printable wall thickness / rod diameter and pore size, improves the freedom of structural design, and provides a new method for the preparation of magnesium alloy porous scaffolds for large bone defects with small pores; at the same time, by adopting a spot compensation strategy based on the size of the molten pool under a specific structure to control the wall thickness / rod diameter, the negative impact of multiple contour scans is eliminated and the size deviation from the model is avoided.

[0047] Other beneficial effects of the present invention will be explained in the specific implementation manner through the introduction of specific technical features and technical solutions. Through the introduction of these technical features and technical solutions, those skilled in the art should be able to understand the beneficial technical effects brought about by the technical features and technical solutions. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0049] Figure 1 The figure is a flow chart of the method of the present invention.

[0050] Figure 2 This is a schematic diagram of the relationship between spot compensation, contour compensation, and fill compensation.

[0051] Figure 3 Schematic diagram of the step effect of slices in LPBF of the present invention and the generation of dross in the overhanging area

[0052] Figure 4 Optical photographs of the top of the stent before and after optimization of the present invention.

[0053] Figure 5 CT scanning results of the cross section of the overhanging region of the stent before and after the contour scanning strategy is optimized according to the present invention. DETAILED DESCRIPTION

[0054] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several changes and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0055] Reference Figure 1 As shown, a method for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface comprises:

[0056] Step 1: Single pass contour scanning and filling scanning to obtain the most compact filling scanning parameters:

[0057] A single contour scan and a single filling scan were performed on the porous scaffold. The contour scan parameters were consistent with the filling scan parameters. After preparation, the sample was cut parallel to the preparation direction, and the cross section was polished to obtain its optical microscopic image and analyze its density. Among the parameter combinations with a density greater than 99.5%, the parameter 0.05≤P / V≤0.5 was selected (P is the laser power in W, V is the scanning speed in mm / s, a smaller V reduces powder splashing, and a smaller P brings a smaller molten pool size to improve accuracy) and set as P 填 、V 填 .

[0058] Step 2, determine the contour scanning strategy with the least powder adhesion, determine the number of pre-contour scans and post-contour scans, contour shrinkage value and fill shrinkage value:

[0059] Fill scan parameter selection P 填 、V 填 , and the contour scanning parameter is set to P 轮 、V 轮 , assuming the number of contour scans is PT (0≤PT≤15), through the formula

[0060]

[0061] To determine the contour scanning parameters, the contour line energy density scaling factor Z = 5 to 30, the value of Z depends on the specific support structure, powder state and filling scanning process and other factors. For example, when Z = 10, PT = 2, P 轮 / V 轮 =0.8*P 填 / V 填 . Contour compensation value PC = (0~2)*S max , Smax The maximum powder particle size, that is, the outer ring profile scanning needs to be able to melt the adhered or agglomerated powder. Figure 2 As shown, within the range of the contour compensation value, both the pre-contour scan (edge ​​scan performed before the fill scan) and the post-contour scan (edge ​​scan performed after the fill scan) can be scanned multiple times, and the scanning sequence is gradually transitioning from the inner circle contour scan to the outer circle contour scan, or from the outer circle contour scan to the inner circle contour scan. Different P, V, PT, Z, and PC can be selected for the pre-contour scan and the post-contour scan. The setting range of the fill compensation value FC is 0≤FC≤PC, which depends on the rod diameter / wall thickness of the prepared stent, the contour scanning power and speed, and the number of contour scans PT.

[0062] Before the filling scan, multiple contour pre-scans with low energy density are set according to the specific support structure and the length of the overhanging area on the lower surface, which can effectively eliminate the slag on the lower surface.

[0063] For porous scaffolds, there is inevitably a lower surface inside. Due to the "step effect" in the model slicing process, there is a certain length of overhanging area on the edge of the model slice. Figure 3 As shown. When the critical forming angle (the angle that requires support, generally 45°) is reached at a specific layer thickness, the length of the overhanging area of ​​the slice increases, resulting in an increase in the length of the laser spot acting on the overhanging area, and ultimately increasing the area of ​​action between the laser and the powder below. Since the powder has a higher absorption rate of laser to the laser than the solidified solid structure, and the thermal conductivity of the powder is lower than that of the solid, the actual heat in the overhanging area is too high, resulting in an increase in the size of the molten pool. In addition, since there is no support below, the molten pool flows into the powder due to gravity, capillary action and the low viscosity of the liquid metal, and the solidified shape is very irregular. This is the dross defect on the lower surface. The formation of dross is mainly caused by excessive local energy input. In order to avoid dross, the molten pool volume needs to be reduced by reducing the energy input of the pre-profile scan for the overhanging structure, but too low energy input will cause unfused defects. Therefore, the number of profile scans needs to be increased to increase the actual energy input, thereby eliminating unfused defects. In the profile scan after the first time, the laser spot acts on the solidified entity, so the molten pool will not be too large, and dross can be avoided in the end. Specific contour compensation value PC 前 , contour scanning times PT 前 It depends on the overhang angle of the lower surface area of ​​the model after slicing and the overhang length between the sliced ​​layers. When the overhang angle is smaller and the overhang length is longer, the supporting effect of the solidified area of ​​the previous layer on the molten pool at the edge of the model is smaller, and a larger contour compensation value PC is required to make the first contour scan act on the solidified entity of the previous layer, and a smaller P 轮 / V 轮Reducing the energy input and the size of the molten pool and more profile scans PT make the edge area dense, and finally make the bracket produce a dross-free lower surface profile.

[0064] After the filling scan, according to the specific surface powder adhesion of the stent, multiple contour scans with low energy density are set to effectively eliminate the surface adhered powder.

[0065] For the incompletely melted powder particles adhering to the top and sides of the support rod after the filling scan, they can be remelted by scanning the contour that expands toward the outer circle of the support rod, so that the powder adhering to the surface of the support rod is melted into a part of the rod diameter, reducing the surface roughness of the support rod, but at the same time it will also increase the wall thickness of the support rod. Due to the unique erosion phenomenon of the LPBF process (erosion refers to the powder-free area along the scanning track, due to the surface tension and the inward airflow caused by the evaporation of the molten pool, the powder particles around the scanning track are adsorbed into the molten pool), there is less powder around the support rod after the filling scan, and no new powder will be melted during the outward offset contour scan. The specific contour compensation value PC 后 , contour scanning times PT 后 It depends on the particle size of the powder and the amount of adhered powder. When the particle size of the adhered powder is larger, a larger offset distance is required to make the light spot act better in the powder; when there are more adhered powders, more scanning times are required to melt the powders into part of the matrix. Therefore, through the low energy density contour post-scanning strategy, the surface powder adhesion can be eliminated and the surface roughness can be reduced.

[0066] Step 3, obtain the molten pool width under the structure and process parameters, and optimize the spot compensation value in a targeted manner:

[0067] The wall thickness / rod diameter T0 of the original design stent model and the wall thickness / rod diameter T1 after the optimized contour scanning strategy are used. The spot compensation value

[0068]

[0069] Where SZ is the spot diameter, R 熔 For the corresponding P 填 / V 填 The molten pool width under cold mounting (obtained by metallographic longitudinal section observation after cold mounting) is adjusted by adjusting the spot compensation value to compensate for the size increase caused by multiple profile scans. For example, T0 = 750μm, T1 = 1000μm, then (T1-T0) / 2 = 125μm, when SZ = 40μm, R 熔 =100μm, R 熔 / SZ=2.5, then

[0070]

[0071] That is, the target rod diameter / wall thickness can be obtained when the spot compensation value SC=50μm.

[0072] Reference Figure 4 As shown, a is the top morphology of the stent before optimization by this method, and b is the top morphology of the stent after optimization by this method. After optimizing the pre-contour scanning strategy and the post-contour scanning strategy, the spot compensation value is adjusted according to the size of the molten pool in the filling scanning area under the specific structure and process parameters, which can effectively reduce the difference between the stent wall thickness and the design value.

[0073] Reference Figure 5 As shown, a is the CT cross-section of the overhanging area of ​​the bracket with slag before optimization using this method, and b is the CT cross-section of the overhanging area of ​​the bracket after optimization using this method. After the powder adhered to the edge of the bracket is re-melted as part of the matrix, the wall thickness / rod diameter will increase to a certain extent. Therefore, it is necessary to set the spot compensation value during slicing to ensure that the wall thickness / rod diameter of the printed bracket is close to the design value. The size of the molten pool has a certain correlation with the structure. The thinner the wall thickness, the worse the thermal conductivity in the vertical direction and the larger the size of the molten pool. Therefore, it is necessary to adjust the spot compensation value specifically according to the size of the molten pool of different structures. (T1-T0) is the wall thickness / rod diameter that needs to be reduced, 2*(R 熔 / SZ) is the reduction in wall thickness when the center of the light spot moves inward by a unit distance under this parameter, and the difference between the two is the light spot compensation value.

[0074] Step 4: Using the optimized contour scanning strategy and spot compensation value, a magnesium alloy tissue engineering scaffold with a wall thickness consistent with the design value, a smooth inner surface and a dense interior is prepared.

[0075] The above are basic embodiments of the present invention. The technical solution of the present invention is further described below through three preferred embodiments.

[0076] Example 1

[0077] Preparation of magnesium stent with minimal curvature

[0078] This embodiment relates to a degradable magnesium alloy tissue engineering scaffold for bone defect repair. Through relevant modeling software, a minimal surface scaffold model with unit type G is designed, the scaffold diameter D = 5mm, the height H = 7mm, the unit size U = 2mm, the model wall thickness T0 = 180μm, and the porosity is about 75%.

[0079] This embodiment relates to a method for preparing the aforementioned high-precision magnesium alloy tissue engineering scaffold with a smooth inner surface, and the method comprises the following steps:

[0080] Step 1: Single-pass contour front scanning and filling scanning to obtain the most compact filling scanning parameters.

[0081] The three-dimensional structure model of the stent was imported into Materialise Mimics software for slicing. After slicing, the data was imported into the 3D printing equipment and printed layer by layer using the ProX DMP 320 metal 3D printer from 3D SYSTEMS of the United States. The powder was a high-purity biodegradable medical magnesium powder with a purity of 99.99%. The shape was a smooth regular sphere with a particle size of 50 to 90 μm and a normal distribution. 平均 =70μm. Before printing, the internal cabin of the 3D printer was repeatedly evacuated and filled with inert gas three times until the oxygen content in the cabin dropped below 30ppm. The spot diameter SZ was set to 80μm, the layer thickness LT was set to 20μm, the scanning spacing HS was set to 80μm, the adjacent layers were rotated 67° for scanning, the contour compensation value PC was set to 0μm, the filling compensation value FC was set to 40μm, and the process window was tried at 100mm / s and 10W. The cross section of the obtained sample was mechanically polished to obtain its metallographic picture, and the density was statistically analyzed (as shown in Table 1). The parameter with a density greater than 99.5% was selected, that is, P 填 =80W, V 填 =500mm / s, the top of the bracket under this parameter is Figure 4 As shown in a.

[0082] Step 2, determine the contour scanning strategy with the least powder adhesion, determine the increase number of contour pre-scanning and contour post-scanning, contour shrinkage value and fill shrinkage value.

[0083] Assume the number of contour scans PT = 6, where the number of contour front scans PT 前 =2, number of post-contour scans PT 后 =4, take Z = 20, then P 轮 / V 轮 =(1-6 / 20)*P 填 / V 填 , fixed V 填 =V 轮 =500mm / s, then P 轮 =0.7*P 填 =56W, take the contour compensation value PC=40μm, the filling compensation FC=40μm, the pre-contour scan is two inner circle contour scans, and the post-contour scan order is first two inner circle contour scans and then two outer circle contour scans.

[0084] Step 3, obtain the molten pool width under the structure and process parameters, and optimize the spot compensation value in a targeted manner.

[0085] Under this profile parameter, the wall thickness of the prepared bracket is T1 = 260 μm. The molten pool width R of the filling scan is obtained by grinding the sample 熔=140μm, then the spot compensation value SC=[(260-180)*80] / (2*140)=22.86μm.

[0086] Step 4: Using the optimized contour scanning strategy and spot compensation value, a magnesium alloy tissue engineering scaffold with a wall thickness consistent with the design value, a smooth surface and a dense interior is prepared.

[0087] The optimized sample preparation parameters are: spot compensation value SC = 32μm, contour compensation value PC = filling compensation FC = 40μm, and the number of scans before contour PT 前 =2, number of post-contour scans PT 后 =4,P 轮 =56W, V 轮 =500mm / s, P 填 =80W, V 填 =500mm / s, and then print again, a magnesium stent with a wall thickness of 180μm and a smooth surface can be prepared. The top of the optimized stent is as follows Figure 4 As shown in b, the obtained scaffold structure has good reproducibility and the surface has a bright metallic luster.

[0088] Table 1 Relationship between different laser powers and scanning speeds and stent density

[0089] 50W 60W 70W 80W 90W 700mm / s 90.70% 92.52% 95.86% 97.94% 98.86% 600mm / s 91.62% 94.93% 97.73% 99.16% 99.52% 500mm / s 92.71% 95.52% 98.97% 99.66% 99.69% 400mm / s 93.63% 97.64% 99.58% 99.87% 99.85% 300mm / s 94.52% 98.99% 99.82% 99.92% 99.98% 200mm / s 95.66% 99.53% 99.73% 99.87% 99.88%

[0090] Example 2

[0091] Preparation of Low-Porosity EK30 Magnesium Alloy Tissue Engineering Scaffold

[0092] This embodiment relates to a degradable gradient scaffold for repairing large bone defects. Through relevant modeling software, a minimal surface scaffold model with unit type G is designed, with a scaffold diameter D=5mm, a height H=3mm, a unit size U=2mm, a model wall thickness T0=450μm, and a porosity of about 50%.

[0093] This embodiment relates to a method for preparing the aforementioned high-precision magnesium alloy bracket with a smooth inner surface, and the method comprises the following steps:

[0094] Step 1: Fill scan and single pass post-contour scan to obtain the most compact fill scan parameters.

[0095] The three-dimensional structure model of the bracket was imported into Materialise Mimics software for slicing. After slicing, the data was imported into the 3D printing equipment and printed layer by layer using the ProX DMP 320 metal 3D printer of 3D SYSTEMS in the United States. The powder was a medical degradable magnesium alloy Mg-3wt.%Nd-0.18wt.%Zn-0.45wt.%Zr, with a smooth regular spherical shape, a particle size of 20 to 50μm, and an average S of 35μm. Before printing, the internal cabin of the 3D printer was repeatedly evacuated and filled with inert gas three times until the oxygen content of the cabin dropped below 30ppm. Set the spot diameter SZ = 60μm, the layer thickness LT = 10μm, the scanning spacing HS = 100μm, rotate the adjacent layers 67° for scanning, set the contour compensation value PC = 0μm, the filling compensation value FC = 40μm, and try the process window in units of 100mm / s and 10W. After mechanically polishing the cross-section of the obtained sample, obtain its metallographic image, and perform density statistics, and select parameters with a density greater than 99.5%, that is, Pfill = 60W, Vfill = 600mm / s.

[0096] Step 2, determine the contour scanning strategy with the least powder adhesion, determine the increase number of contour pre-scanning and contour post-scanning, contour shrinkage value and fill shrinkage value.

[0097] Assume the number of contour scans PT = 8, where the number of contour front scans PT 前 =4, number of post-contour scans PT 后 =4, take Z = 24, then P 轮 / V 轮 =(1-8 / 24)*P 填 / V 填 , fixed V 填 =V 轮 =600mm / s, then P 轮 =2 / 3*Pfill=40W, take contour compensation value PC=20μm, filling compensation FC=20μm, the pre-contour scan is first two outer circle contour scans, then two inner circle contour scans, the post-contour scan is first two inner circle contour scans, then two outer circle contour scans.

[0098] Step 3, obtain the molten pool width under the structure and process parameters, and optimize the spot compensation value in a targeted manner.

[0099] Under this profile parameter, the wall thickness of the prepared bracket is T1 = 500 μm. The molten pool width R of the filling scan is obtained by grinding the sample 熔 =80μm, then the spot compensation value SC=[(500-450)*60] / (2*80)=18.75μm.

[0100] Step 4: Using the optimized contour scanning strategy and spot compensation value, a magnesium alloy tissue engineering scaffold with a wall thickness consistent with the design value, a smooth surface and a dense interior is prepared.

[0101] The optimized sample preparation parameters are: spot compensation value SC = 18.75 μm, contour compensation value PC = filling compensation FC = 20 μm, and the number of scans before contour PT 前 =4, number of post-contour scans PT 后 =4,P 轮 =40W, V wheel = 600mm / s, P 填 =60W, V 填 = 600mm / s, and printing is performed again, then a magnesium bracket with a wall thickness of 450μm and no dross in the overhang area can be prepared. The cross section of the bracket overhang area before and after the optimization of the contour scanning strategy is shown in Figure 2. Figure 5 shown.

[0102] Example 3

[0103] Preparation of Diamond-structured WE43 Magnesium Alloy Tissue Engineering Scaffolds

[0104] This embodiment relates to a degradable gradient scaffold for repairing large bone defects. A rod-shaped diamond structure scaffold model is designed through relevant modeling software, with a scaffold diameter of D = 10 mm, a height of H = 15 mm, a unit size of U = 1.2 mm, a model rod diameter T0 = 760 μm, and a porosity of about 60%.

[0105] This embodiment relates to a method for preparing the aforementioned high-precision magnesium alloy tissue engineering scaffold with a smooth inner surface, and the method comprises the following steps:

[0106] Step 1: Single-pass contour front scanning and filling scanning to obtain the most compact filling scanning parameters.

[0107] The three-dimensional structure model of the bracket was imported into Materialise Mimics software for slicing. After slicing, the data was imported into the 3D printing equipment and printed layer by layer using the ProX DMP 320 metal 3D printer of 3D SYSTEMS in the United States. The powder was WE43 commercial magnesium alloy powder with a purity of 99.99%, a smooth regular spherical shape, a particle size of 40 to 80 μm, and a normal distribution, S average = 60 μm. Before printing, the internal cabin of the 3D printer was repeatedly evacuated and filled with inert gas three times until the oxygen content of the cabin dropped below 30 ppm. Set the spot diameter SZ = 70μm, the layer thickness LT = 30μm, the scanning spacing HS = 120μm, rotate the adjacent layers 67° for scanning, set the contour compensation value PC = 0μm, the filling compensation value FC = 30μm, and try the process window in units of 100mm / s and 10W. After mechanically polishing the cross section of the obtained sample, obtain its metallographic image, and perform density statistics, select parameters with a density greater than 99.5%, Pfill = 90W, Vfill = 500mm / s.

[0108] Step 2, determine the contour scanning strategy with the least powder adhesion, determine the increase number of contour pre-scanning and contour post-scanning, contour indentation value and filling indentation value. Assume the contour scanning number PT = 7, where the contour pre-scanning number PT 前 =1, number of scans after contour PT 后 =6, take Z = 21, then P 轮 / V 轮 =(1-7 / 21)*P 填 / V 填 , fixed V 填 =V 轮 =500mm / s, then P 轮 =2 / 3*P 填 =60W, take the contour compensation value PC=30μm, the filling compensation FC=30μm, the pre-contour scan is first one inner circle contour scan, the post-contour scan is first three outer circle contour scans, and then three inner circle contour scans.

[0109] Step 3, obtain the molten pool width under the structure and process parameters, and optimize the spot compensation value in a targeted manner. Under this profile parameter, the rod diameter of the prepared bracket is T1 = 920 μm. The molten pool width R of the filling scan is obtained by grinding the sample 熔

[0110] =130μm, then the spot compensation value SC=[(920-760)*70] / (2*130)=43.08μm.

[0111] Step 4: Using the optimized contour scanning strategy and spot compensation value, a magnesium alloy tissue engineering scaffold with a wall thickness consistent with the design value, a smooth surface and a dense interior was prepared. The optimized sample preparation parameters were: spot compensation value SC = 43.08 μm, contour compensation value PC = filling compensation FC = 30 μm, and the number of pre-contour scans PT 前 =1, number of scans after contour PT 后 =6,P 轮 =40W, V 轮 =600mm / s, P 填 =90W, V 填 =500mm / s, and printing is performed again to produce a diamond-structured WE43 magnesium alloy tissue engineering scaffold with a rod diameter of 760μm and no slag in the overhanging area.

[0112] In summary, the advantages of the present invention are that it can eliminate the powder sticking and slag defects that seriously affect the inner surface roughness and the performance of the scaffold in the complex porous structure in situ during the preparation process, thereby improving the fluidity, fatigue and corrosion resistance of the porous scaffold, simplifying the cumbersome post-processing process, reducing production costs, and realizing the concept of green production. It greatly broadens the maximum printable size of the porous scaffold, reduces the minimum printable wall thickness / rod diameter and pore diameter, and improves the freedom of structural design, providing a new method for the preparation of magnesium alloy porous scaffolds for large bone defects with small pores. At the same time, by adopting a spot compensation strategy based on the size of the molten pool under a specific structure to control the wall thickness / rod diameter, the negative impact of multiple contour scanning is eliminated, and the size deviation from the model is avoided.

[0113] The present invention also provides a system for preparing an LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface. The system for preparing an LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface can be realized by executing the process steps of the method for preparing an LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface, that is, those skilled in the art can understand the method for preparing an LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface as a preferred implementation of the system for preparing an LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface.

[0114] Specifically, a system for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface comprises:

[0115] Module M1: Scan the porous scaffold and select the most dense filling scanning parameters;

[0116] The scanning includes a single-pass contour scan and a single-pass fill scan;

[0117] Module M2: Optimize the contour scanning strategy based on the most dense filling scanning parameters;

[0118] Module M3: Obtain the corresponding molten pool size and adjust the spot compensation value using the optimized contour scanning strategy;

[0119] Module M4: Preparation of magnesium alloy tissue engineering scaffolds based on contour scanning strategy and adjusted spot compensation value.

[0120] The module M1 comprises:

[0121] The porous scaffold was subjected to a single contour scan and a single filling scan. The contour scan parameters were consistent with the filling scan parameters. After preparation, the sample was cut parallel to the preparation direction. The cross section was polished to obtain its optical microscopic image and analyze its density. Among the parameter combinations with a density greater than 99.5%, the parameter with 0.05≤P / V≤0.5 was selected and set as P 填 、V 填 ;

[0122] Where P is the laser power and V is the scanning speed.

[0123] The module M2 comprises:

[0124] Select fill scan parameter as P 填 、V 填 , let the contour scanning parameter be P 轮 、V 轮 , the number of contour scans is PT, and the contour parameters are calculated:

[0125]

[0126] Among them, the contour line energy density scaling factor Z=5~30, within the range of the contour compensation value, the contour pre-scan and contour post-scan can be scanned multiple times, and the scanning sequence includes from the inner circle contour scanning to the outer circle contour scanning, or from the outer circle contour scanning to the inner circle contour scanning; the contour pre-scan and contour post-scan can select different laser powers P, scanning speeds V, contour scanning times PT, contour line energy density scaling factors Z and contour compensation values ​​PC; the setting range of the filling compensation value FC is 0≤FC≤PC.

[0127] The module M3 comprises:

[0128] Obtain the molten pool width under the structure and process parameters, and optimize the spot compensation value;

[0129] Assume that the wall thickness / rod diameter of the original design stent model is T0, and the wall thickness / rod diameter after the optimized contour scanning strategy is T1, then the spot compensation value is:

[0130]

[0131] Where SZ is the spot diameter, R 熔 For the corresponding P 填 / V 填 The size increase caused by multiple contour scans is compensated by adjusting the spot compensation value.

[0132] The module M1 also includes setting multiple pre-contour scans with a certain energy density before filling scans according to the specific stent structure and the length of the lower surface overhang area; and setting multiple post-contour scans with a certain energy density after filling scans according to the specific surface powder adhesion of the stent.

[0133] Those skilled in the art know that, in addition to realizing the system and its various devices, modules, and units provided by the present invention in a purely computer-readable program code, it is entirely possible to realize the same functions in the form of logic gates, switches, application-specific integrated circuits, programmable logic controllers, and embedded microcontrollers by logically programming the method steps. Therefore, the system and its various devices, modules, and units provided by the present invention can be considered as a hardware component, and the devices, modules, and units included therein for realizing various functions can also be regarded as structures within the hardware component; the devices, modules, and units for realizing various functions can also be regarded as both software modules for realizing the method and structures within the hardware component.

[0134] In the description of the present application, it should be understood that the terms "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0135] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various changes or modifications within the scope of the claims, which does not affect the essence of the present invention. In the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other arbitrarily.

Claims

1. A method for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface, characterized in that: include: Step S1: Scan the porous scaffold to select the most dense filling scanning parameters; The scanning includes a single-pass contour scan and a single-pass fill scan; Step S2: Optimizing the contour scanning strategy according to the most dense filling scanning parameters; Step S3: Obtain the corresponding molten pool size and adjust the spot compensation value using the optimized contour scanning strategy; Step S4: preparing a magnesium alloy tissue engineering scaffold based on the contour scanning strategy and the adjusted spot compensation value.

2. The method for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface according to claim 1, characterized in that: The step S1 comprises: The porous scaffold was subjected to a single contour scan and a single filling scan. The contour scan parameters were consistent with the filling scan parameters. After preparation, the sample was cut parallel to the preparation direction. The cross section was polished to obtain its optical microscopic image and analyze its density. Among the parameter combinations with a density greater than 99.5%, the parameter with 0.05≤P / V≤0.5 was selected and set as P 填 、V 填 ; Where P is the laser power and V is the scanning speed.

3. The method for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface according to claim 2, characterized in that: The step S2 comprises: Select fill scan parameter as P 填 、V 填 , let the contour scanning parameter be P 轮 、V 轮 , the number of contour scans is PT, and the contour parameters are calculated: Among them, the contour line energy density scaling factor Z=5~30, within the range of the contour compensation value, the contour pre-scan and contour post-scan can be scanned multiple times, and the scanning sequence includes from the inner circle contour scanning to the outer circle contour scanning, or from the outer circle contour scanning to the inner circle contour scanning; the contour pre-scan and contour post-scan can select different laser powers P, scanning speeds V, contour scanning times PT, contour line energy density scaling factors Z and contour compensation values ​​PC; the setting range of the filling compensation value FC is 0≤FC≤PC.

4. The method for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface according to claim 3, characterized in that: The step S3 comprises: Obtain the molten pool width under the structure and process parameters, and optimize the spot compensation value; Assume that the wall thickness / rod diameter of the original design stent model is T0, and the wall thickness / rod diameter after the optimized contour scanning strategy is T1, then the spot compensation value is: Where SZ is the spot diameter, R 熔 For the corresponding P 填 / V 填 The size increase caused by multiple contour scans is compensated by adjusting the spot compensation value.

5. The method for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface according to claim 2, characterized in that: The step S1 also includes setting multiple pre-contour scans with a certain energy density according to the specific stent structure and the length of the lower surface overhang area before the filling scan; and setting multiple post-contour scans with a certain energy density according to the surface powder adhesion of the specific stent after the filling scan.

6. A method for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface, characterized in that: include: Module M1: Scan the porous scaffold and select the most dense filling scanning parameters; The scanning includes a single-pass contour scan and a single-pass fill scan; Module M2: Optimize the contour scanning strategy based on the most dense filling scanning parameters; Module M3: Obtain the corresponding molten pool size and adjust the spot compensation value using the optimized contour scanning strategy; Module M4: Preparation of magnesium alloy tissue engineering scaffolds based on contour scanning strategy and adjusted spot compensation value.

7. The method for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface according to claim 6, characterized in that: The module M1 comprises: The porous scaffold was subjected to a single contour scan and a single filling scan. The contour scan parameters were consistent with the filling scan parameters. After preparation, the sample was cut parallel to the preparation direction. The cross section was polished to obtain its optical microscopic image and analyze its density. Among the parameter combinations with a density greater than 99.5%, the parameter with 0.05≤P / V≤0.5 was selected and set as P 填 、V 填 ; Where P is the laser power and V is the scanning speed.

8. The method for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface according to claim 7, characterized in that: The module M2 comprises: Select fill scan parameter as P 填 、V 填 , let the contour scanning parameter be P 轮 、V 轮 , the number of contour scans is PT, and the contour parameters are calculated: Among them, the contour line energy density scaling factor Z=5~30, within the range of the contour compensation value, the contour pre-scan and contour post-scan can be scanned multiple times, and the scanning sequence includes from the inner circle contour scanning to the outer circle contour scanning, or from the outer circle contour scanning to the inner circle contour scanning; the contour pre-scan and contour post-scan can select different laser powers P, scanning speeds V, contour scanning times PT, contour line energy density scaling factors Z and contour compensation values ​​PC; the setting range of the filling compensation value FC is 0≤FC≤PC.

9. The method for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface according to claim 8, characterized in that: The module M3 comprises: Obtain the molten pool width under the structure and process parameters, and optimize the spot compensation value; Assume that the wall thickness / rod diameter of the original design stent model is T0, and the wall thickness / rod diameter after the optimized contour scanning strategy is T1, then the spot compensation value is: Where SZ is the spot diameter, R 熔 For the corresponding P 填 / V 填 The size increase caused by multiple contour scans is compensated by adjusting the spot compensation value.

10. The method for preparing a LPBF magnesium alloy tissue engineering scaffold with a smooth inner surface according to claim 7, characterized in that: The module M1 also includes setting multiple pre-contour scans with a certain energy density before filling scans according to the specific stent structure and the length of the lower surface overhang area; and setting multiple post-contour scans with a certain energy density after filling scans according to the specific surface powder adhesion of the stent.

Citation Information

Cited By

  • Method for controlling powder sticking phenomenon of porous metal in laser additive manufacturing

    CN120755356A

  • Fabrication method and system for LPBF magnesium-alloy tissue-engineering scaffold with smooth inner surface

    WO2026031699A1