Method for preparing lithium sulfide by taking lithium-containing ore as raw material
By preparing lithium sulfide from lithium-containing ores, using crystal-form transformation roasting, acidization roasting and multi-stage purification processes, combined with spray pyrolysis and sintering technology, the problems of high environmental protection costs and harsh process conditions in the existing lithium sulfide preparation process are solved. , realize the preparation of low-cost and high-purity lithium sulfide.
Patent Information
- Application Number
- CN202411103832.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The use of hydrogen sulfide and organic solvents in the existing lithium sulfide preparation process leads to high environmental protection costs and harsh process conditions, making it difficult to implement on a large scale.
Lithium-containing ore is used as raw material, and lithium sulfate refined liquid is obtained through crystalline transformation calcination, acidification calcination, leaching and multi-stage purification. Combined with soluble organic carbon dissolution and spray pyrolysis, and finally, high-purity lithium sulfide is sintered under an inert atmosphere.
It significantly reduces the preparation cost, improves the purity of lithium sulfide, avoids the use of hydrogen sulfide and organic solvents, simplifies process conditions, and reduces environmental protection costs.
Smart Images

Figure CN118992981A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of new materials and new energy technologies, and relates to a method for preparing lithium sulfide using lithium-containing ore as a raw material. Technical Background
[0002] Lithium sulfide is the core material of sulfide all-solid-state secondary battery technology. According to the aggregation form of reactants, its technical routes can be divided into four types: all-solid phase, gas-solid phase, solid-liquid phase and all-liquid phase.
[0003] After summarizing and analyzing, it is found that almost all gas-phase reactions are provided with sulfur source by hydrogen sulfide, and almost all liquid-phase reactions contain organic solvents. Due to the highly toxic nature of hydrogen sulfide and the flammability and explosiveness of organic solvents, the safety and environmental protection costs of these two types of reactions are high. In addition, some technical routes are difficult to implement due to environmental protection policies. At the same time, the prices of some organic lithium salts are too high and are limited to small sample preparation in the laboratory.
[0004] Solid phase reaction avoids the use of hydrogen sulfide and organic solvents, thus significantly reducing environmental costs. However, when single lithium and lithium hydride are used as reaction raw materials, the phase reaction process is extremely intense, heat generation is serious, and it is difficult to control because these materials have strong reactivity. At the same time, the hydrogen generated by lithium hydride has the risk of explosion. This type of reaction has extremely demanding requirements for process conditions and equipment conditions. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing lithium sulfide using lithium-containing ore as raw material to solve the deficiencies in the prior art. The unit preparation cost of lithium sulfide is significantly reduced and the purity of the product is significantly improved by using the preparation process provided by the present invention.
[0006] To achieve the above object, a method for preparing lithium sulfide using lithium-containing ore as raw material, wherein the lithium-containing ore includes one or more of spodumene, pyroxenite, and lepidolite; the method comprises the following steps:
[0007] (1) subjecting lithium-containing ore to crystal transformation roasting, acid roasting, leaching, and multi-stage purification in sequence to obtain a lithium sulfate refined solution;
[0008] (2) fully dissolving the soluble organic carbon in the refined lithium sulfate solution to obtain a precursor slurry;
[0009] (3) preparing a precursor powder by spray pyrolysis of the obtained precursor slurry;
[0010] (4) Sintering the precursor powder under an inert atmosphere to obtain high-purity lithium sulfide.
[0011] The crystal transformation roasting is to roast the lithium-containing ore at a temperature above 1000°C for 30-300 minutes; the acidification roasting is to mix the ore powder into concentrated sulfuric acid and roast it at a temperature above 200°C for more than 10 minutes to obtain roasted clinker. The crystal transformation roasting is to ensure that the concentrated sulfuric acid can better leach lithium elements, such as spodumene, in the later stage; but this step can be omitted for lepidolite and pyroxenite.
[0012] The leaching process involves soaking the acidified and roasted lithium-containing ore in water, and filtering and separating the lithium sulfate-containing mother liquor. After the spodumene undergoes the early crystal transformation and sulfation roasting, the roasted clinker mainly contains lithium sulfate, which is dissolved into the liquid phase through the neutralization and water leaching process, wherein the lithium sulfate concentration is 100-200 g / L. However, the impurity content in the leaching solution is relatively high, and it must be purified and impurities removed.
[0013] The multi-stage purification is to add calcium carbonate to remove iron and aluminum elements. Through calcium carbonate neutralization, the pH of the leaching end point is controlled to 6.5 to remove most of the aluminum and iron. However, the inability to remove alkaline earth metals such as calcium and magnesium will still affect the quality of the subsequent preparation of lithium carbonate, and the leachate must be purified and impurities removed.
[0014] Sodium hydroxide is added to remove magnesium, and sodium carbonate is added to remove calcium.
[0015] The lithium sulfate purified liquid thus obtained has a lithium sulfate purity greater than 99% based on the solid material precipitated by evaporation and crystallization.
[0016] The soluble organic carbon includes one or more of glucose, sucrose, fructose, maltose and citric acid.
[0017] The atomization method of the spray pyrolysis is one of pressure spray and centrifugal spray; the inlet air temperature is between 180-240° C., and the outlet air temperature is set between 100-150° C. This inlet air temperature can make the organic carbon source initially decompose, so as to reduce the reaction waste gas emission and improve the product yield.
[0018] The inert atmosphere is nitrogen atmosphere, argon atmosphere or vacuum; the heating rate of sintering is 2-4°C / min, and the temperature is kept at 700-1000°C for 5-10h.
[0019] The carbon thermal reduction method is an important technical route for preparing lithium sulfide, but the high cost of raw materials leads to the high cost of lithium sulfide produced by this technical route. Therefore, the traditional preparation route of directly extracting lithium sulfate refined liquid from ore without the need for re-sulfation of lithium carbonate and omitting the drying step significantly reduces the cost of raw materials.
[0020] As an efficient means of material preparation, spray drying has significant advantages in solving the segregation of soluble reactants, reaction morphology and particle size control. Consider dissolving the soluble carbon source directly in the refined lithium sulfate solution, using the spray drying process, and using the form of spray granulation to tightly wrap the lithium sulfate particles on the surface of the water-insoluble carbon particles to achieve the effect of uniform mixing and full contact of the reaction surface. Through sintering, high-purity lithium sulfide can be directly obtained without subsequent purification. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A flow chart for preparing a lithium sulfate refined solution from a lithium-containing ore, and then preparing lithium sulfide based on the lithium sulfate refined solution;
[0022] Figure 2 This is the phase diagram of lithium sulfide prepared in Examples 1 to 3. DETAILED DESCRIPTION
[0023] The physical characterization and electrolyte preparation and characterization of the embodiment are as follows:
[0024] Phase characterization: All XRD tests were performed using the PANalytical Empyrean high-intensity X-ray diffractometer from the Netherlands, and the XRD standard card library was PDF2004. Since lithium sulfide is unstable to air, all tests were performed using PI tape wrapping. All lithium oxide impurity peaks tested were test errors and were not taken into account.
[0025] Preparation and characterization of electrolyte: Lithium sulfide, phosphorus pentasulfide, and lithium chloride were added to a zirconia ball mill according to the designed ratio, and ball milled for 1 hour at a ball-to-material ratio of 40:1 to obtain electrolyte raw powder; the raw powder was sintered at 500°C for 8 hours to obtain electrolyte powder. A certain amount of electrolyte powder was made into a blocked cell with a diameter of 10 mm under a pressure of 300 MPa, and then the impedance test module of the electrochemical workstation was used to test the impedance spectrum in the frequency range of 1 to 1 MHz to obtain the electrolyte impedance, which was converted into conductivity according to the thickness.
[0026] Example 1
[0027] The spodumene ore roasted at 1150℃ was crushed to 135μm, and 97% concentrated sulfuric acid was added to the acidified rotary kiln for roasting at 1200℃ for 2h, and then the ore was taken out of the kiln for cooling; then deionized water was added at a concentration of 1kg / L to soak the acidified roasted ore for 60min, and filtered to obtain a lithium precipitation mother liquor. Then calcium carbonate was added in turn, filtered to obtain a primary lithium precipitation mother liquor; sodium hydroxide was added, filtered to obtain a secondary lithium precipitation mother liquor; sodium carbonate was added, filtered, and finally a lithium sulfate refined liquid with a concentration of about 200g / L was obtained.
[0028] 140 g of glucose was added to the above-mentioned lithium sulfate refined liquid, and stirred to obtain a clarified slurry.
[0029] The obtained slurry was pumped into the spray dryer by a peristaltic pump. The air inlet temperature was set to 195°C, the air outlet temperature was set to 120°C, and the precursor powder was obtained by spraying. All the powders were put into a bowl, and the temperature was increased to 825°C at a heating rate of 1.2°C / min in a flowing nitrogen atmosphere, kept at this temperature for 8 hours, and cooled to obtain high-purity lithium sulfide powder.
[0030] Take the above lithium sulfide, prepare electrolyte according to the raw material ratio of Li2S:P2S5:LiCl=5:1:2, and test the conductivity.
[0031] Example 2
[0032] The lithium mica ore is crushed into 155μm, and 95% concentrated sulfuric acid is added to the acidified rotary kiln for roasting at 1100℃ for 2h, and then the ore is taken out of the kiln for cooling; then deionized water is added at a concentration of 0.5kg / L to soak the acidified roasted ore for 60min, and filtered to obtain a lithium precipitation mother liquor. Then calcium carbonate is added in turn, filtered to obtain a primary lithium precipitation mother liquor; sodium hydroxide is added, filtered to obtain a secondary lithium precipitation mother liquor; sodium carbonate is added, filtered, and finally a lithium sulfate refined liquid with a concentration of about 120g / L is obtained.
[0033] 100 g of citric acid was added to the above-mentioned lithium sulfate refined liquid, and stirred to obtain a clarified slurry.
[0034] The obtained slurry was pumped into the spray dryer by a peristaltic pump. The air inlet temperature was set to 225°C, the air outlet temperature was set to 110°C, and the precursor powder was obtained by spraying. All the powders were put into a bowl, and the temperature was increased to 975°C at a heating rate of 2.0°C / min in a flowing nitrogen atmosphere, kept at this temperature for 8 hours, and cooled to obtain high-purity lithium sulfide powder.
[0035] Take the above lithium sulfide, prepare electrolyte according to the raw material ratio of Li2S:P2S5:LiCl=5:1:2, and test the conductivity.
[0036] Example 3
[0037] The phosphate lithium aluminum stone is crushed to 180μm, and 98% concentrated sulfuric acid is added to the acidified rotary kiln for roasting at 1200℃ for 2h, and then the ore is taken out of the kiln for cooling; then deionized water is added at a concentration of 2kg / L to soak the acidified roasted ore for 30min, and filtered to obtain a lithium precipitation mother liquor. Then calcium carbonate is added in sequence, filtered to obtain a primary lithium precipitation mother liquor; sodium hydroxide is added, filtered to obtain a secondary lithium precipitation mother liquor; sodium carbonate is added, filtered, and finally a lithium sulfate refined liquid with a concentration of about 100g / L is obtained.
[0038] 100 g of sucrose was added to the above-mentioned lithium sulfate refined liquid, and stirred to obtain a clarified slurry.
[0039] The obtained slurry was pumped into a spray dryer using a peristaltic pump. The air inlet temperature was set to 205°C, the air outlet temperature was set to 150°C, and the precursor powder was obtained by spraying. All the powders were put into a bowl, and the temperature was increased to 850°C at a rate of 2.5°C / min in a flowing nitrogen atmosphere, kept at this temperature for 2 hours, and cooled to obtain high-purity lithium sulfide powder.
[0040] Take the above lithium sulfide, prepare electrolyte according to the raw material ratio of Li2S:P2S5:LiCl=5:1:2, and test the conductivity.
[0041] Table 1
[0042]
[0043] The purity of lithium sulfide obtained in Examples 1-3 and the conductivity of the prepared electrolyte are shown in Table 1, from which it can be seen that the present invention can directly prepare lithium sulfide from lithium-containing ore, the raw material cost is extremely low, the product purity reaches more than 99%, and the conductivity of the prepared electrolyte reaches more than 4mS / cm.
[0044] In summary, the scheme of the present invention takes raw material cost control as the starting point, starts from low-cost lithium-containing ore, and after continuous optimization and purification, combined with spray drying and high-temperature sintering processes, finally obtains high-quality lithium sulfide.
[0045] In view of the many defects of the prior art, the inventor of this case, after long-term research and extensive practice, proposed the technical solution of the present invention, and further explained the technical solution, its implementation process and principle, etc. However, it should be understood that within the scope of the present invention, the above-mentioned technical features of the present invention and the technical features specifically described in the above (embodiment) can be combined with each other to form a new or preferred technical solution.
[0046] Unless otherwise specified, the materials, reagents, etc. used in the above examples can be obtained from commercial sources.
Claims
1. A method for preparing lithium sulfide using lithium-containing ore as raw material, characterized in that: The lithium-containing ore includes one or more of spodumene, pyroxenite, and lepidolite; the method includes the following steps: (1) subjecting a lithium-containing ore to acid roasting, leaching, and multi-stage purification to obtain a lithium sulfate refined solution; wherein, when the lithium-containing ore is spodumene, before the acid roasting, the lithium-containing ore is roasted through crystal transformation; (2) fully dissolving the soluble organic carbon in the refined lithium sulfate solution to obtain a precursor slurry; (3) preparing a precursor powder by spray pyrolysis of the obtained precursor slurry; (4) Sintering the precursor powder under an inert atmosphere to obtain high-purity lithium sulfide.
2. The method according to claim 1, characterized in that: The crystal transformation roasting is to roast the lithium-containing ore at above 1000°C for 30-300 minutes; the acidification roasting is to mix the ore powder into concentrated sulfuric acid and roast it at above 200°C for more than 10 minutes.
3. The method according to claim 1, characterized in that The leaching process is to soak the acidified and roasted lithium-containing ore in water, and filter and separate the lithium sulfate-containing mother liquor, wherein the lithium sulfate concentration is 100-200 g / L.
4. The method according to claim 1, characterized in that The multi-stage purification is to remove the iron and aluminum elements by adding calcium carbonate, remove the magnesium element by adding sodium hydroxide, and remove the calcium element by adding sodium carbonate.
5. The method according to claim 1, characterized in that The soluble organic carbon includes one or more of glucose, sucrose, fructose, maltose and citric acid.
6. The method according to claim 1, characterized in that The atomization mode of the spray pyrolysis is one of pressure spray and centrifugal spray, the inlet air temperature is between 180-240°C, and the outlet air temperature is set between 100-150°C.
7. The method according to claim 1, characterized in that The inert atmosphere is nitrogen atmosphere, argon atmosphere or vacuum; the heating rate of sintering is 2-4°C / min, and the temperature is kept at 700-1000°C for 5-10h.
Citation Information
Patent Citations
Method for extracting lithium in slag produced through recycling of lithium battery by pyrogenic process
CN108063295A
Method used for producing lithium sulfate mother liquor or lithium carbonate by taking spodumene as raw material
CN108423694A
Method of preparing and purifying lithium sulfide
CN111908431A
Method for preparing lithium hydroxide from spodumene
CN116873953A
Method for preparing lithium carbonate by utilizing amblygonite
CN117003264A
Cited By
Method for preparing high-purity lithium sulfide based on lithium sulfate solution for extracting lithium from lithium ore and sulfide solid electrolyte
CN119976745A
Method for preparing high-purity lithium sulfide from lithium sulfate solution based on lithium ore lithium extraction and sulfide solid electrolyte
CN119976745B
Lithium sulfide composite material and preparation method thereof
CN120749213A