High-capacity resin / asphalt-based hard carbon negative electrode material and preparation method thereof, negative electrode plate and sodium ion battery
Through the preparation method of resin/asphalt-based hard carbon negative electrode material, the cross-linking curing process and soft carbon coating process are used to optimize the structure and interface of hard carbon material, and the problem of low efficiency of hard carbon negative electrode material for the first time is solved, achieving high capacity and Stable cycle performance and reduce costs.
Patent Information
- Application Number
- CN202411086594.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
The first Coulombic efficiency of hard carbon anode material is mainly due to the instability of the precursor structure and interface defects, which lead to irreversible reactions and irreversible capacity.
Using the preparation method of resin/asphalt-based hard carbon negative electrode material, the resin-based hard carbon precursor is formed through preoxidation and carbonization treatment, and sintered in an inert atmosphere, and the cross-linking curing process and soft carbon coating process are introduced to optimize the material Structural and interface characteristics.
The first Coulomb efficiency and reversible capacity of hard charcoal materials are improved, high capacity is maintained, and material costs are reduced, and stable cycling performance is achieved.
Smart Images

Figure CN118993024A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a high-capacity resin / asphalt-based hard carbon negative electrode material and a preparation method thereof, a negative electrode sheet and a sodium ion battery. Background Art
[0002] Due to the abundant sodium reserves and low price, sodium-ion batteries are considered to be one of the most promising energy storage methods in the future. Carbon materials are low-cost, widely available, and have stable physical and chemical properties, and are used in the negative electrode of sodium-ion batteries. Among them, hard carbon as a sodium-ion battery electrode material has a high low-voltage platform capacity and is one of the most promising negative electrode materials for sodium-ion batteries. Hard carbon precursors are widely available, and biomass, resin, coal, high molecular polymers, etc. can all be used as hard carbon raw materials.
[0003] Although the disordered structure of hard carbon is very suitable for storing large-sized sodium ions and has achieved a high capacity, there are still some problems, such as low first coulombic efficiency. The low first coulombic efficiency of hard carbon is mainly caused by two aspects: first, the large specific surface area caused by the unstable precursor structure, the sodium ions and the decomposed electrolyte will produce an irreversible reaction to form an electrolyte interface film (SEI) covering the surface of the negative electrode material; second, the large number of interface defects will cause sodium ions to be irreversibly embedded in some active sites. This will produce irreversible capacity.
[0004] Therefore, how to optimize the structure and interface of hard carbon negative electrode materials so as to improve the first coulombic efficiency of hard carbon materials while maintaining high capacity has become an urgent problem to be solved. Summary of the invention
[0005] In order to overcome the technical problem in the prior art that it is difficult for the negative electrode material to have the first coulombic efficiency of the hard carbon material while maintaining high capacity due to the structure and interface of the hard carbon negative electrode material, the purpose of the present invention is to provide a high-capacity resin / asphalt-based hard carbon negative electrode material and a preparation method, a negative electrode sheet and a sodium ion battery, wherein the negative electrode material has.
[0006] To achieve the above objectives, the technical solutions implemented in this plan are as follows:
[0007] A method for preparing a high-capacity resin / asphalt-based hard carbon negative electrode material comprises the following steps:
[0008] The resin, curing agent, solvent and dopant are mixed and then pre-oxidized to obtain a cross-linked product;
[0009] The cross-linked product is carbonized to obtain a resin-based hard carbon precursor;
[0010] The asphalt, the resin-based hard carbon precursor and the organic solvent are mixed and dried to obtain a composite hard carbon precursor;
[0011] The composite hard carbon precursor is sintered in an inert atmosphere to obtain a resin / asphalt-based hard carbon negative electrode material.
[0012] Furthermore, the resin is selected from one or a combination of phenolic resin, urea-formaldehyde resin, epoxy resin, silicone resin, polyester resin, furfural resin, polyamide resin, bismaleimide resin and polyimide resin.
[0013] Furthermore, the curing agent is selected from one or a combination of maleic anhydride, ethylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, diethylaminopropylamine and phthalic anhydride.
[0014] Furthermore, the solvent used when mixing the resin, curing agent, solvent and dopant is selected from one or a combination of water, isopropanol, ethanol, ethylene glycol and n-butanol; the dopant is one or a combination of elemental sulfur, phosphoric acid, boric acid, silicic acid, manganese chloride and diammonium phosphate.
[0015] Further, the mass ratio of resin, curing agent, solvent and dopant is 40-80:1-4:20:0-0.6;
[0016] The temperature for mixing the resin, curing agent, solvent and dopant is 25°C to 60°C; the pre-oxidation treatment temperature is 150°C to 220°C, and the pre-oxidation treatment time is 4 to 12 hours.
[0017] Furthermore, the carbonization temperature is 500-800° C., and the time is 4-12 hours.
[0018] Furthermore, the asphalt is one or a combination of coal tar asphalt, petroleum asphalt and natural asphalt; the organic solvent is one or a combination of ethanol, isopropanol, tetrahydrofuran, carbon tetrachloride, N-methylpyrrolidone and N,N-dimethylformamide.
[0019] Furthermore, the mass ratio of the resin-based hard carbon precursor to the asphalt is 1 to 5:1; the inert atmosphere is one or a combination of nitrogen, argon, helium and neon; the sintering temperature is 1100°C to 1400°C, and the time is 2 to 4 hours.
[0020] A negative electrode sheet comprises the negative electrode material prepared by the method.
[0021] A sodium ion battery comprises a positive electrode, an electrolyte and the negative electrode sheet.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] In the present invention, resin-based hard carbon is used as a precursor material, so the resin-based hard carbon material has the characteristics of high specific capacity and excellent batch stability. The purpose of cross-linking is achieved by mixing resin, curing agent, solvent and dopant and then subjecting them to pre-oxidation treatment. The cross-linked product is carbonized to achieve the purpose of curing. A cross-linking curing process is introduced. By adding a cross-linking agent and a solvent in a mixture of resin, curing agent, solvent and dopant as a pore-forming agent, the proportion of effective closed pores and pore size parameters in the resin-based hard carbon precursor are adjusted to enable it to have a high first-cycle discharge capacity. By mixing asphalt, resin-based hard carbon precursor and organic solvent After mixing and drying, a soft carbon coating process is introduced. The soft carbon has high electrical conductivity and toughness. When the asphalt is coated with the resin-based hard carbon precursor, the soft carbon can block some open holes in the resin-based hard carbon precursor on the one hand, and on the other hand, it can also reduce the surface defects and specific surface area of the resin-based hard carbon precursor, thereby inhibiting the formation of a solid electrolyte interface and obtaining stable cycle performance and high reversible capacity. The sintering process is optimized in the present invention, and a carbonization and sintering, i.e., a two-step carbonization process is designed. Compared with the sintering process of resin-based hard carbon materials, a lower carbonization temperature can be selected for material preparation after coating the soft carbon.
[0024] Furthermore, the raw materials for preparing the hard carbon material in the present invention are phenolic resin and asphalt, which are abundant and widely available, and asphalt is low in cost. The prepared hard carbon negative electrode material maintains the characteristics of high capacity and high initial efficiency when used as the negative electrode of a sodium ion battery. Compared with the preparation process of resin-based hard carbon, the preparation method of the present invention is simple and effectively reduces the cost of materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a first-week discharge curve of a half-cell prepared with a hard carbon negative electrode according to Example 1 of the present invention;
[0026] Figure 2 This is a microscopic morphology of the resin / asphalt-based hard carbon negative electrode material prepared in an embodiment of the present invention. DETAILED DESCRIPTION
[0027] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thoroughly and comprehensively understood.
[0028] The present invention provides a method for preparing a high-capacity resin / asphalt-based hard carbon negative electrode material, comprising the following steps:
[0029] S1: mixing resin, solvent, curing agent and dopant in a mass ratio of 40-80:20:1-4:0-0.6, stirring thoroughly and placing in a high-temperature blast oven for pre-oxidation treatment to obtain a cross-linked product;
[0030] S2: After mechanically crushing the cross-linked product in step S1, the first step of high-temperature carbonization treatment is performed, and the sintered product is ball-milled and sieved to obtain a resin-based hard carbon precursor;
[0031] S3: mixing the asphalt, the resin-based hard carbon precursor and the organic solvent in a mass ratio of 1:2:5-8 and stirring them fully, evaporating the solvent and then drying to obtain a composite hard carbon precursor;
[0032] S4: placing the composite hard carbon precursor obtained in step S3 in an inert atmosphere for a second high-temperature sintering, cooling and sieving to obtain a resin / asphalt-based hard carbon negative electrode material.
[0033] Preferably, in step S1, the resin is selected from one or more combinations of phenolic resin, urea-formaldehyde resin, epoxy resin, silicone resin, polyester resin, furfural resin, polyamide resin, bismaleimide resin and polyimide resin; the curing agent is selected from one or more combinations of maleic anhydride, ethylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, diethylaminopropylamine and phthalic anhydride; the solvent is selected from one or more combinations of water, isopropanol, ethanol, ethylene glycol and n-butanol; the dopant is one or more combinations of elemental sulfur, phosphoric acid (mass concentration is 85%), boric acid, silicic acid, manganese chloride and diammonium phosphate.
[0034] Preferably, the temperature for mixing the components in step S1 is 25° C. to 60° C.; the pre-oxidation treatment temperature is 150° C. to 220° C.; and the pre-oxidation treatment time is 4 to 12 hours.
[0035] Preferably, the temperature of the first high-temperature carbonization in step S2 is 500-800° C., and the time is 4-12 hours; the speed of the ball mill is 400-600 r / min, and the ball milling time is 4-12 hours.
[0036] Preferably, the asphalt in step S3 is one or a combination of coal tar asphalt, petroleum asphalt and natural asphalt, and the organic solvent is selected from one or a combination of ethanol, isopropanol, tetrahydrofuran, carbon tetrachloride, N-methylpyrrolidone (NMP) and N,N-dimethylformamide (DMF); the mass ratio of the resin-based hard carbon precursor to the asphalt is 1 to 5:1.
[0037] Preferably, the inert atmosphere selected for sintering in step S4 is one or a combination of nitrogen, argon, helium and neon; the sintering temperature is 1100° C. to 1400° C., and the holding time is 2 to 4 hours.
[0038] The present invention also provides a high-capacity resin / asphalt-based hard carbon negative electrode material prepared by the above preparation method.
[0039] The present invention also provides a negative electrode sheet prepared from the negative electrode material.
[0040] The present invention also provides a sodium ion battery, comprising the negative electrode sheet.
[0041] The following are specific embodiments.
[0042] Example 1
[0043] 40g of phenolic resin was mixed with 20g of isopropanol, 2g of maleic anhydride and 0.6g of phosphoric acid. After stirring evenly, it was placed in a blast oven for 6h. After being taken out, it was crushed. The crushed cross-linked product was placed in a tubular furnace and carbonized at 600℃ for 6h under nitrogen atmosphere. After being taken out, it was ball milled at a speed of 400r / min for 4h. After ball milling, it was sieved through a 350-mesh sieve to obtain a resin-based hard carbon precursor. The resin-based hard carbon precursor, asphalt and acetone were fully stirred at a mass ratio of 2:1:5. After stirring evenly, it was placed in a blast oven at 100℃ for drying to obtain a resin / asphalt composite precursor. The composite precursor was placed in a tubular furnace for the second step of high-temperature sintering. Nitrogen was introduced as a protective atmosphere. The sintering temperature was 1400℃ and the insulation time was 2h. The sintered product was sieved through a 300-mesh sieve to obtain a resin / asphalt-based hard carbon composite material. Its microscopic morphology is shown in FIG. Figure 1 , it can be seen that the hard carbon particles are uniform in size, ranging from 5 to 15 μm, and their morphology is irregular blocks, and the surface of the material is evenly coated.
[0044] After testing, the first discharge capacity of the half-cell prepared by the hard carbon negative electrode is 395.10mAh·g-1, the first efficiency is 85.5%, and the first week discharge curve is shown in Figure 2 .
[0045] Example 2
[0046] 40 g of phenolic resin was mixed with 20 g of ethanol, 2 g of maleic anhydride and 0.6 g of phosphoric acid. After stirring evenly, it was placed in a blast oven for insulation for 8 h. After being taken out, it was crushed. The crushed cross-linked product was placed in a tubular furnace and carbonized at 600 ° C for 6 h under nitrogen atmosphere. After being taken out, it was ball milled at a speed of 400 r / min for 4 h. After ball milling, it was sieved through a 350-mesh sieve to obtain a resin-based hard carbon precursor; the resin-based hard carbon precursor, asphalt and NMP were fully stirred at a mass ratio of 2:1:8, stirred evenly and placed in a blast oven at 100 ° C to dry to obtain a resin / asphalt composite precursor. The composite precursor was placed in a tubular furnace for the second step of high-temperature sintering. Nitrogen was introduced as a protective atmosphere. The sintering temperature was 1300 ° C and the insulation time was 2 h. The sintered product was sieved through a 300-mesh sieve to obtain a resin / asphalt-based hard carbon composite material. After testing, the half-cell prepared with the hard carbon negative electrode had an initial discharge capacity of 390.79 mAh·g-1 and an initial efficiency of 86.75%.
[0047] Example 3
[0048] 40g of phenolic resin was mixed with 20g of ethanol, 2g of maleic anhydride and 0.6g of phosphoric acid, stirred evenly and put into a blast oven for insulation for 8h. After being taken out, the product was crushed and the crushed cross-linked product was put into a tubular furnace for high-temperature carbonization at 600℃ for 4h under nitrogen atmosphere. After being taken out, the product was ball milled at a speed of 400r / min for 2h. After ball milling, the product was sieved through a 300-mesh sieve to obtain a resin-based hard carbon precursor. The resin-based hard carbon precursor, asphalt and carbon tetrachloride solution were fully stirred at a mass ratio of 2:1:5, stirred evenly and put into a blast oven at 100℃ for drying to obtain a resin / asphalt composite precursor. The composite precursor was put into a tubular furnace for the second step of high-temperature sintering. Nitrogen was introduced as a protective atmosphere. The sintering temperature was 1200℃ and the insulation time was 3h. The sintered product was sieved through a 300-mesh sieve to obtain a resin / asphalt-based hard carbon composite material. After testing, the half-cell prepared with the hard carbon negative electrode had an initial discharge capacity of 380.18 mAh·g-1 and an initial efficiency of 85.85%.
[0049] Example 4
[0050] 40g of phenolic resin was mixed with 20g of ethanol, 2g of maleic anhydride, 0.6g of phosphoric acid and 0.08g of manganese chloride, stirred evenly and put into a blast oven for insulation for 8h. After being taken out, the product was crushed. The crushed cross-linked product was put into a tubular furnace and carbonized at 600℃ for 6h under argon atmosphere. After being taken out, the product was ball milled at a speed of 400r / min for 4h. After ball milling, the product was sieved through a 350-mesh sieve to obtain a resin-based hard carbon precursor. The resin-based hard carbon precursor, asphalt and acetone were fully stirred at a mass ratio of 2:1:5, stirred evenly and put into a blast oven at 100℃ for drying to obtain a resin / asphalt composite precursor. The composite precursor was put into a box furnace for the second step of high-temperature sintering. Argon was introduced as a protective atmosphere. The sintering temperature was 1200℃ and the insulation time was 4h. The sintered product was sieved through a 300-mesh sieve to obtain a resin / asphalt-based hard carbon composite material. After testing, the half-cell prepared with the hard carbon negative electrode had an initial discharge capacity of 374.10 mAh·g-1 and an initial efficiency of 84.50%.
[0051] Example 5
[0052] 40 g of bisphenol A epoxy resin was mixed with 20 g of ethanol and 2 g of maleic anhydride, stirred evenly, and then placed in a blast oven for insulation for 8 hours. The product was taken out and crushed, and the crushed cross-linked product was placed in a tubular furnace and carbonized at 600°C for 6 hours under nitrogen atmosphere. The product was taken out and ball milled at a speed of 400 r / min for 4 hours. After ball milling, the product was sieved through a 350-mesh sieve to obtain a resin-based hard carbon precursor. The resin-based hard carbon precursor, asphalt, and NMP were mixed in a mass ratio of 2:1:8, and the mixed liquid was heated and stirred until the solvent was evaporated to obtain a resin / asphalt composite precursor. The composite precursor was placed in a tubular furnace for the second step of high-temperature sintering. Nitrogen was introduced as a protective atmosphere. The sintering temperature was 1300°C and the insulation time was 2 hours. The sintered product was sieved through a 300-mesh sieve to obtain a resin / asphalt-based hard carbon composite material. After testing, the half-cell prepared with the hard carbon negative electrode had an initial discharge capacity of 356.89 mAh·g-1 and an initial efficiency of 87.83%.
[0053] Example 6
[0054] 40g of urea-formaldehyde resin, 20g of water, 2g of phthalic anhydride, 0.3g of manganese chloride and 0.3 of ammonium dihydrogen phosphate were mixed at 25°C, stirred evenly and put into a blast oven at 160°C for 10h, taken out and crushed, the crushed cross-linked product was put into a tubular furnace, carbonized at 650°C for 6h under nitrogen atmosphere, taken out and ball milled at a speed of 600r / min for 4h, and passed through a 350-mesh sieve to obtain a resin Based hard carbon precursor; the resin-based hard carbon precursor, asphalt, acetone, and DMF are fully stirred in a mass ratio of 5:1:4:1, and after stirring evenly, they are placed in a 100°C blast oven for drying to obtain a resin / asphalt composite precursor, and the composite precursor is placed in a tubular furnace for the second step of high-temperature sintering, and nitrogen is introduced as a protective atmosphere. The sintering temperature is 1100°C and the insulation time is 4h. The sintered product is sieved through a 300-mesh sieve to obtain a resin / asphalt-based hard carbon composite material.
[0055] Example 7
[0056] 50g of epoxy resin, 20g of ethylene glycol, 2g of triethylenetetramine, 2g of diethylaminopropylamine and 0.1g of manganese chloride were mixed at 60°C, stirred evenly and put into a blast oven at 200°C for 6h, taken out and crushed, the crushed cross-linked product was put into a tubular furnace, carbonized at 700°C for 5h under nitrogen atmosphere, taken out and ball milled at a speed of 500r / min for 10h, and passed through a 350-mesh sieve to obtain a resin Based hard carbon precursor; the resin-based hard carbon precursor, asphalt, and DMF are fully stirred in a mass ratio of 2:1:5, and after stirring evenly, they are placed in a 100°C blast oven for drying to obtain a resin / asphalt composite precursor, and the composite precursor is placed in a tubular furnace for the second step of high-temperature sintering, and a mixture of nitrogen and neon is introduced as a protective atmosphere. The sintering temperature is 1400°C and the insulation time is 2h. The sintered product is sieved through a 300-mesh sieve to obtain a resin / asphalt-based hard carbon composite material.
[0057] Example 8
[0058] 60g of silicone resin, 20g of polyester resin, 20g of n-butanol, 3g of diethylenetriamine and 0.2g of silicic acid are mixed at 30°C, stirred evenly, and then placed in a blast oven at 180°C for 8h. After being taken out, the product is crushed, and the crushed cross-linked product is placed in a tubular furnace, carbonized at 600°C for 7h under nitrogen atmosphere. After being taken out, it is ball milled at a speed of 600r / min for 4h. After ball milling, it is sieved through a 350-mesh sieve to obtain a resin-based hard carbon precursor; the resin-based hard carbon precursor, asphalt and tetrahydrofuran are fully stirred at a mass ratio of 3:1:5, stirred evenly, and then placed in a blast oven at 100°C for drying to obtain a resin / asphalt composite precursor. The composite precursor is placed in a tubular furnace for the second step of high-temperature sintering, neon gas is introduced as a protective atmosphere, the sintering temperature is 1300°C, the insulation time is 3h, and the sintered product is sieved through a 300-mesh sieve to obtain a resin / asphalt-based hard carbon composite material.
[0059] Example 9
[0060] 70g furfural resin, 20g polyamide resin, 10g isopropanol, 10g n-butanol, 2g hexamethylenediamine and 0.3g boric acid were mixed at 40°C, stirred evenly and put into a blast oven at 220°C for 4h, taken out and crushed, the crushed cross-linked product was put into a tubular furnace, carbonized at 800°C for 4h under nitrogen atmosphere, taken out and ball milled at a speed of 400r / min for 12h, and passed through 350 mesh after ball milling. The resin-based hard carbon precursor is obtained by sieving; the resin-based hard carbon precursor, asphalt and isopropanol are fully stirred in a mass ratio of 4:1:5, and after stirring evenly, they are placed in a 100°C blast oven for drying to obtain a resin / asphalt composite precursor, and the composite precursor is placed in a tubular furnace for the second step of high-temperature sintering, and helium is introduced as a protective atmosphere. The sintering temperature is 1250°C and the insulation time is 3h. The sintered product is sieved through a 300-mesh sieve to obtain a resin / asphalt-based hard carbon composite material.
[0061] Example 10
[0062] 80g of bismaleimide resin, 20g of polyimide resin, 20g of isopropanol, 1g of ethylenediamine and 0.4g of sulfur were mixed at 50°C, stirred evenly and put into a blast oven at 150°C for 12h, taken out and crushed, and the crushed cross-linked product was put into a tube furnace and carbonized at 500°C for 12h under nitrogen atmosphere, taken out and ball milled at a speed of 450r / min for 10h, and then milled for 350 mesh sieve to obtain a resin-based hard carbon precursor; the resin-based hard carbon precursor, asphalt and ethanol are fully stirred in a mass ratio of 5:1:5, and after stirring evenly, they are put into a 100°C blast oven for drying to obtain a resin / asphalt composite precursor; the composite precursor is placed in a tubular furnace for the second step of high-temperature sintering, argon is introduced as a protective atmosphere, the sintering temperature is 1350°C, the insulation time is 2h, and the sintered product is passed through a 300-mesh sieve to obtain a resin / asphalt-based hard carbon composite material.
[0063] Comparative Example 1
[0064] The sodium-electric hard carbon is made from commercial biomass from Japan Kuraray Company, model: Type-1
[0065] The physical and chemical properties of Examples 1-5 and the comparative example were tested in accordance with the national standard GBT-24533-2019 "Graphite Anode Materials for Lithium-ion Batteries". The test results are shown in Table 1.
[0066] The examples 1-5 and the comparative example are used as the negative electrode materials for sodium ion batteries to assemble button cells. The preparation method of the negative electrode materials is as follows: the prepared resin / asphalt-based hard carbon negative electrode material powder, carbon black, carboxymethyl cellulose solution, and SBR binder are mixed in a mass ratio of 80:10:4:6 to form a slurry, and then the slurry is evenly scraped onto the current collector copper foil, dried, and cut into The battery was assembled in a glove box with an argon atmosphere, with sodium metal as the counter electrode and 1.0M NaPF6 in EC:DMC; EMC = 1:1:1 Vol%. The electrochemical performance was tested on a Wuhan Blue Electric CT2001A battery tester with a charge and discharge voltage range of 0V to 3V. The test results are shown in Table 1.
[0067] Table 1 Electrochemical performance test results
[0068]
[0069] It can be seen from Table 1 that the battery prepared by the present invention has the characteristics of high capacity and high initial efficiency.
[0070] The above description is only for the best embodiment of the present invention, but it should not be understood as limiting the claims. The present invention is not limited to the above embodiments, and its specific structure is allowed to be changed. However, all changes made within the protection scope of the independent claims of the present invention are within the protection scope of the present invention.
[0071] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
Claims
1. A method for preparing a high-capacity resin / asphalt-based hard carbon negative electrode material, characterized in that: The following steps are involved: The resin, curing agent, solvent and dopant are mixed and then pre-oxidized to obtain a cross-linked product; The cross-linked product is carbonized to obtain a resin-based hard carbon precursor; The asphalt, the resin-based hard carbon precursor and the organic solvent are mixed and dried to obtain a composite hard carbon precursor; The composite hard carbon precursor is sintered in an inert atmosphere to obtain a resin / asphalt-based hard carbon negative electrode material.
2. The method for preparing a high-capacity resin / asphalt-based hard carbon negative electrode material according to claim 1, characterized in that: The resin is selected from one or a combination of phenolic resin, urea-formaldehyde resin, epoxy resin, silicone resin, polyester resin, furfural resin, polyamide resin, bismaleimide resin and polyimide resin.
3. The method for preparing a high-capacity resin / asphalt-based hard carbon negative electrode material according to claim 1, characterized in that: The curing agent is selected from one or a combination of maleic anhydride, ethylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, diethylaminopropylamine and phthalic anhydride.
4. The method for preparing a high-capacity resin / asphalt-based hard carbon negative electrode material according to claim 1, characterized in that: The solvent for mixing the resin, curing agent, solvent and dopant is selected from one or a combination of water, isopropanol, ethanol, ethylene glycol and n-butanol; the dopant is one or a combination of elemental sulfur, phosphoric acid, boric acid, silicic acid, manganese chloride and diammonium phosphate.
5. The method for preparing a high-capacity resin / asphalt-based hard carbon negative electrode material according to claim 1, characterized in that: The mass ratio of resin, curing agent, solvent and dopant is 40-80:1-4:20:0-0.6; The temperature for mixing the resin, curing agent, solvent and dopant is 25°C to 60°C; the pre-oxidation treatment temperature is 150°C to 220°C, and the pre-oxidation treatment time is 4 to 12 hours.
6. The method for preparing a high-capacity resin / asphalt-based hard carbon negative electrode material according to claim 1, characterized in that: The carbonization temperature is 500-800°C and the time is 4-12 hours.
7. The method for preparing a high-capacity resin / asphalt-based hard carbon negative electrode material according to claim 1, characterized in that the asphalt It is one or a combination of coal tar pitch, petroleum pitch and natural pitch; the organic solvent is one or a combination of ethanol, isopropanol, tetrahydrofuran, carbon tetrachloride, N-methylpyrrolidone and N,N-dimethylformamide.
8. The method for preparing a high-capacity resin / asphalt-based hard carbon negative electrode material according to claim 1, characterized in that: The mass ratio of the resin-based hard carbon precursor to the asphalt is 1 to 5:1; the inert atmosphere is one or a combination of nitrogen, argon, helium and neon; the sintering temperature is 1100° C. to 1400° C., and the sintering time is 2 to 4 hours.
9. A negative electrode sheet, characterized in that: A negative electrode material prepared by the method according to any one of claims 1 to 8.
10. A sodium ion battery, characterized in that: The invention comprises a positive electrode, an electrolyte and the negative electrode sheet as claimed in claim 9.
Citation Information
Patent Citations
Preparation method of soft carbon coated hard carbon negative electrode material for lithium ion battery
CN111900400A
Hard carbon composite material and preparation method and application thereof
CN113880068A
Soft carbon coated phosphorus / sodium co-doped hard carbon sodium ion battery negative electrode material and preparation method thereof
CN118315549A
Cited By
Hard carbon material and preparation method thereof, negative pole piece and battery
CN119240664A
Preparation method of hard carbon doped with pre-oxidized heavy organic matter in situ
CN119430148A
A hard carbon negative electrode material and preparation method thereof and sodium ion battery
CN119750549A
Preparation method and application of low-rank coal-based hard carbon material
CN119954132A
Asphalt-based hard carbon negative electrode material for sodium-ion battery and preparation method of asphalt-based hard carbon negative electrode material
CN120081362A