Ultra-stable high-entropy metal oxide electrode capable of being used for alternating current pole reversal
By using ultra-stable high-entropy metal oxide electrodes in high-salt wastewater treatment, the electrocatalytic cathode scaling problem is solved, the corrosion resistance and corrosion resistance of the electrode are improved, and the efficient electrocatalytic process is achieved, and energy consumption is reduced. and maintenance costs.
Patent Information
- Application Number
- CN202411413186.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-10-11
AI Technical Summary
The electrocatalytic cathode is prone to scaling problems in high-salt wastewater treatment, which leads to a decrease in current efficiency, increased energy consumption and shortened service life, affecting the pollutant removal effect.
Ultra-stable high-entropy metal oxide electrode is adopted to form an anti-corrosion carbide layer through ion implantation technology, and a high-entropy alloy surfactant layer is formed by mechanical alloying treatment, and a gradient grain structure is formed by high-energy laser direct energy deposition method and plasma treatment. Finally, nanotitanium dioxide coating and doped molybdenum ions are prepared on the electrode to achieve AC inverter to prevent scaling.
It significantly improves the corrosion resistance and corrosion resistance of the electrode, avoids cathode scaling, reduces energy consumption and maintenance costs, and improves the stability and efficiency of the electrocatalytic process.
Smart Images

Figure CN118993256A_ABST
Abstract
Description
1. Technical Field
[0001] The present invention relates to the field of environmental pollution control technology, and in particular to an ultrastable high entropy metal oxide electrode that can be used for alternating current reversal. In view of the fact that the cathode scaling problem of the electrocatalytic electrode seriously restricts the application of electrocatalysis in the treatment of high-salt and high-hardness wastewater, the electrocatalytic electrode that can be frequently reversed is of great significance in the industrial application field of electrocatalytic technology. 2. Background Technology
[0002] High-salinity wastewater comes from a wide range of sources, mainly including chemical, pharmaceutical, printing and dyeing, seawater desalination and food processing industries. Its output is huge and is on the rise with the development of industry. High-salinity wastewater has significant characteristics. It contains a large amount of inorganic salts, such as sodium chloride, sodium sulfate, etc., and may also contain a variety of organic matter and heavy metals. Its salinity is usually above 3.5%, or even higher. High-salinity wastewater is seriously harmful to the environment. Direct discharge will cause soil salinization, affect vegetation growth and crop yields; after entering the water body, it will increase the salinity of the water body, destroy the balance of the aquatic ecosystem, and affect the survival and reproduction of aquatic organisms. In addition, organic matter and heavy metals in high-salinity wastewater may also accumulate in the environment, be transmitted through the food chain, and pose a potential threat to human health. The treatment of high-salinity wastewater is difficult and is one of the important challenges facing environmental protection.
[0003] In the field of deep treatment of high-salinity wastewater, common treatment technologies include membrane separation, ion exchange, advanced oxidation and evaporative crystallization. Membrane separation technology can efficiently separate impurities and produce good effluent quality, but the membrane is easily contaminated, has high requirements for influent quality and needs regular cleaning and replacement, which increases operating costs; ion exchange technology can selectively remove specific ions, is simple to operate, and occupies a small area of equipment, but the resin needs to be regenerated, and the regeneration process produces wastewater and is easily saturated with high-concentration salt water; advanced oxidation technology can produce strong oxidizing free radicals, has good removal effect on difficult-to-degrade organic matter, fast reaction speed and no secondary pollution, but has high operating costs, some oxidants are unstable and have strict requirements on reaction conditions; evaporative crystallization technology can achieve salt recovery and zero wastewater discharge, and the treatment effect is stable and suitable for high-salinity wastewater, but it has high energy consumption and large equipment investment, and the crystallized product needs further treatment to avoid secondary pollution.
[0004] Electrocatalysis is widely used in the deep treatment of high-salinity wastewater. Its main technical advantages are mild reaction conditions, simple operation, and efficient removal of organic matter and some heavy metal ions in wastewater. The high salinity in high-salinity wastewater can increase the conductivity of the solution and reduce the energy consumption of the electrocatalytic process. However, electrocatalysis also has defects in treating high-salinity wastewater, especially when the hardness of the water is high, the cathode is prone to scaling. The reaction mechanism of cathode scaling is mainly that calcium, magnesium and other ions in the water combine with hydroxide ions on the cathode surface to form insoluble precipitates such as calcium carbonate and magnesium hydroxide. The chemical composition of the scaling layer is mainly calcium carbonate, magnesium hydroxide, etc., and its thickness will gradually increase with the operating time. The scaling layer will have many adverse effects on the electrocatalytic process, such as reducing the effective surface area of the electrode, resulting in a decrease in current efficiency; increasing the resistance between electrodes, increasing energy consumption; affecting the stability and service life of the electrode, and increasing maintenance costs. At the same time, the scaling layer may also hinder the contact between pollutants and the electrode surface, reducing the removal effect of organic matter and heavy metals.
[0005] Analyzing the existing problems in the current electrocatalytic deep treatment of high-salinity wastewater, it is urgent to develop new technical methods to prevent the problem of electrocatalytic cathode scaling. This will be conducive to improving the efficiency and stability of electrocatalytic deep treatment of high-salinity wastewater. By reducing cathode scaling, the current efficiency of the electrode can be improved, energy consumption can be reduced, and the continuous and stable operation of the treatment process can be guaranteed. This will help to achieve the standard discharge or resource recycling of high-salinity wastewater, promote industrial sustainable development, and protect the ecological environment. At the same time, the research and development of new methods will also bring technological innovation to the field of high-salinity wastewater treatment and provide strong support for solving the problems of water shortage and environmental pollution. III. Summary of the invention
[0006] The present invention is made in view of the problems existing in the prior art. Generally speaking, cathode scaling can be alleviated by physical, chemical and electrochemical methods. For example, scaling can be reduced by optimizing the electrode structure and designing special electrodes, but this generally increases costs and process complexity; ultrasonic treatment requires additional equipment and has high energy consumption. In chemical methods, adding scale inhibitors such as polyphosphates, organic phosphonic acids, etc. can form complexes with calcium and magnesium ions to prevent precipitation, but new chemicals may be introduced to affect wastewater treatment; adjusting the pH value needs to consider the impact on the pollutant treatment effect.
[0007] The main principle of cathode-cathode reversal to prevent electrochemical scaling is to periodically change the polarity of the electrode so that the scaling material originally deposited on the cathode is dissolved or converted under the anode polarity, thereby preventing the continuous accumulation of scaling. Taking the common scaling of calcium and magnesium ions as an example, in the normal electrocatalytic process, the cathode reaction will increase the concentration of hydroxide ions in the water, and calcium and magnesium ions will combine with hydroxide to form calcium carbonate (CaCO3) and magnesium hydroxide (Mg(OH)2) precipitation. The reaction formula is:
[0008] Ca 2 ++2OH-→CaCO3+H2O
[0009] Mg2++2OH-→Mg(OH)2
[0010] After the cathode is reversed, the original cathode becomes the anode, and calcium carbonate and magnesium hydroxide will undergo oxidation reaction at the anode and dissolve. This can effectively prevent the long-term accumulation of scale on the electrode, maintain the performance of the electrode and the stability of the electrocatalytic process. For example, calcium carbonate may react:
[0011] CaCO3+2H + →Ca 2 ++CO2+H2O
[0012] But the current problem is that the common commercial anode materials, such as ruthenium iridium, lead oxide, tin oxide, nickel oxide, etc., cannot withstand long-term cathode current, which may cause inevitable damage to the electrode. Therefore, there is an urgent need to develop metal oxide electrodes that can be used for AC reversal and have high stability, high activity and selectivity.
[0013] In order to achieve the above-mentioned object, the technical solution of the present invention is an ultrastable high entropy metal oxide electrode that can be used for AC reversal, characterized in that the preparation method of the electrode comprises the following steps:
[0014] Step 1, the tantalum substrate is subjected to high-precision polishing treatment to make its surface roughness reach Ra 0.5μm, and then the polished tantalum substrate is placed in an ultrasonic cleaner, cleaned with acetone for 15 minutes to remove surface oil, then rinsed with deionized water, and then immersed in a dilute hydrochloric acid solution with a mass concentration of 5% for 15 minutes to remove surface oxides, and finally rinsed with deionized water and dried at a drying temperature of 100°C for 30 minutes;
[0015] Step 2: Use ion implantation technology to form an ultra-stable anti-corrosion carbide layer. The implanted ions are titanium carbide ions and zirconium carbide ions. The implantation energy is 120 keV and the implantation dose is 8×10 16 ions cm -2 The injection process was carried out under a vacuum of 1×10 -3 The process was carried out in a Pa environment, with an injection temperature of 150°C and an injection time of 10 s to obtain a tantalum substrate with an ultra-stable anti-corrosion carbide layer;
[0016] Step 3: Select 7 metal powders of tantalum, rubidium, gadolinium, dysprosium, chromium, nickel and cadmium according to the molar ratio of 120:7:16:22:9:2:1, and put the prepared raw materials into a planetary ball mill for mechanical alloying treatment at a speed of 400 rpm. –1The ball-to-material ratio was 15:1, the ball milling time was 20 h, and argon protection was introduced during the ball milling process to prevent metal oxidation. The powder after ball milling was kept at a vacuum degree of 1×10 –2 Heat treatment was carried out in a vacuum environment of 1.5 Pa at a temperature of 800°C for 2 h to obtain a mixed powder of 7 metals;
[0017] Step 4: Use argon as carrier gas to spray the mixed powder of the seven metals obtained in step 3 at a speed of 20 L / min. –1 The nozzle temperature was 1200°C, and the powder was sprayed line by line on the tantalum substrate with an ultra-stable anti-corrosion carbide layer obtained in step 2 after ion implantation. At the same time, the high-energy laser direct energy deposition method was used to melt the high-entropy alloy powder on the tantalum substrate to form a high-entropy alloy surface active layer. The laser power was 15 kW and the scanning speed was 0.5 mm s –1 The overlap rate is 40%, and the cladding process is carried out under argon protection; the deposited high entropy alloy will produce a gradient grain structure with alternating growth of equiaxed crystals and columnar crystals due to cyclic heat input and rapid solidification;
[0018] Step 5, plasma treatment and ceramicization are performed on the surface active layer of the high entropy alloy after laser cladding obtained in step 4 to improve its surface activity and corrosion resistance. The plasma treatment uses a mixed gas of argon and oxygen, wherein the volume fraction of oxygen is 10%, the treatment power is 300w, the treatment time is 20min, and the treatment temperature is 50°C, so as to convert the high entropy alloy layer into a high entropy ceramic layer;
[0019] Step 6, a nano titanium dioxide coating is prepared on the high entropy ceramic layer obtained in step 5 by a sol-gel method. First, butyl titanate, ethanol, acetylacetone and deionized water are mixed in a mass ratio of 8:2:10:1, stirred evenly to obtain a sol, and then the electrode is immersed in the sol at 4 mm min –1 Repeated pulling, drying in air and then heat treatment at 450°C for 2h;
[0020] Step 7. Finally, the electrode is modified by ion doping technology to improve its electrocatalytic activity and selectivity. Molybdenum ions are selected for doping. The doping mass concentration is 3%. The doping method is electrochemical deposition. The deposition voltage is -1.0V. The deposition process is carried out in an ammonium molybdate electrolyte containing a mass concentration of 20%. The electrolyte temperature is 40°C. After the deposition time is 30 minutes, the electrode is taken out and washed with deionized water to obtain an ultra-stable high-entropy metal oxide electrode that can be used for AC reversal.
[0021] The present invention is beneficial in that:
[0022] 1) Excellent anti-corrosion performance: An ultra-stable anti-corrosion carbide layer is formed on the tantalum substrate through ion implantation technology. Titanium carbide ions and zirconium carbide ions are implanted under specific vacuum, temperature and energy conditions, which greatly improves the anti-corrosion ability of the electrode and prolongs the service life of the electrode in harsh environments.
[0023] 2) Unique high-entropy alloy formula and preparation method: Seven metal element powders, including tantalum, rubidium, gadolinium, dysprosium, chromium, nickel and cadmium, are selected and mixed in a specific molar ratio. Mechanical alloying treatment is carried out using a planetary ball mill and heat treatment is carried out under specific conditions. Argon carrier gas injection and high-energy laser direct energy deposition are then used to form a high-entropy alloy surface active layer, produce a gradient grain structure, and enhance the performance of the electrode.
[0024] 3) Enhanced surface activity and corrosion resistance: The surface active layer of the high-entropy alloy is plasma treated and ceramicized. A mixed gas of argon and oxygen is used at a specific power, time and temperature to convert the high-entropy alloy layer into a high-entropy ceramic layer. At the same time, a sol-gel method is used to prepare a nano-titanium dioxide coating, which further improves the surface activity and corrosion resistance of the electrode.
[0025] 4) AC reversal can be used to prevent scaling and save costs: The electrode can be reversed by AC, and will not be affected during the reversal process. It can effectively prevent the scaling of calcium and magnesium ions in high-salt wastewater on the electrode, saving a lot of reagents and labor costs, and providing an efficient and economical solution for high-salt wastewater treatment. IV. Description of the drawings
[0026] In order to more clearly illustrate the specific embodiments of the present invention, the drawings used in the description of the specific embodiments are briefly described below. Figure 1 The scale formation on the surface of the ultrastable high entropy metal oxide electrode that can be used for AC reversal under the conditions of AC reversal frequencies of 20 Hz (a), 10 Hz (b), 0.1 Hz (c), and 0 Hz (d) (scanning electron microscopy).
[0027] Figure 2 The change of exchange current intensity over time of the ultrastable high entropy metal oxide electrode that can be used for AC reversal under the conditions of AC reversal frequencies of 20Hz, 10Hz, 0.1Hz, and 0Hz.
[0028] Figure 3 The figure shows the changes in the surface electrochemical impedance spectroscopy (EIS) spectrum of an ultrastable high entropy metal oxide electrode that can be used for AC reversal under the conditions of AC reversal frequencies of 20 Hz, 10 Hz, 0.1 Hz, and 0 Hz.
[0029] Figure 4The ultrastable high entropy metal oxide electrode that can be used for AC reversal shows the change of calcium ion concentration with reaction time in solutions with different initial calcium ion concentrations under 20Hz AC reversal conditions.
[0030] Figure 5 The degradation process of landfill leachate by commercially available lead oxide electrodes in batches at an AC reversal frequency of 20 Hz, and the variation of electrode activity with the degradation batches.
[0031] Figure 6 The process of batch degradation of landfill leachate by an ultrastable high entropy metal oxide electrode that can be used for AC reversal at an AC reversal frequency of 20 Hz is presented, and the variation of electrode activity with the degradation batches.
[0032] Figure 7 The process of batch degradation of fracturing flowback fluid by ultrastable high entropy metal oxide electrodes that can be used for AC reversal at an AC reversal frequency of 20 Hz is shown, and the changes in electrode activity along the degradation batches. V. Specific implementation methods
[0033] The present invention is described in detail below with reference to the accompanying drawings and embodiments:
[0034] Embodiment 1:
[0035] An ultra-stable high-entropy metal oxide electrode that can be used for alternating current reversal is characterized in that the preparation method of the electrode comprises the following steps: firstly, a tantalum substrate is subjected to high-precision grinding treatment to make its surface roughness reach Ra 0.5 μm, then the ground tantalum substrate is placed in an ultrasonic cleaner, and is cleaned with acetone for 15 minutes to remove surface oil stains, then rinsed with deionized water, and then immersed in a dilute hydrochloric acid solution with a mass concentration of 5% for 15 minutes to remove surface oxides, and finally rinsed with deionized water and dried, the drying temperature is 100°C, and the time is 30 minutes; an ultra-stable anti-corrosion carbide layer is formed by ion implantation technology, the implanted ions are titanium carbide ions and zirconium carbide ions, the implantation energy is 120 keV, and the implantation dose is 8×10 16 ions cm –2 The injection process was carried out under a vacuum of 1×10 –3 Pa environment, the injection temperature was 150 ° C, the injection time was 10s, and a tantalum substrate with an ultra-stable anti-corrosion carbide layer was obtained; 7 metal element powders of tantalum, rubidium, gadolinium, dysprosium, chromium, nickel, and cadmium were selected and mixed according to the molar ratio of 120:7:16:22:9:2:1, and the mixed raw materials were placed in a planetary ball mill for mechanical alloying treatment, and the ball mill speed was 400 rpm –1 The ball-to-material ratio was 15:1, the ball milling time was 20 h, and argon protection was introduced during the ball milling process to prevent metal oxidation. The powder after ball milling was kept at a vacuum degree of 1×10 –2Pa vacuum environment, the heat treatment temperature was 800 ° C, the time was 2 h, and the mixed powder of 7 metals was obtained; the mixed powder of 7 metals was sprayed at a speed of 20 L min using argon as carrier gas. –1 The nozzle temperature was 1200°C, and the laser was sprayed line by line on the tantalum substrate with an ultra-stable anti-corrosion carbide layer after ion implantation. At the same time, the high-energy laser direct energy deposition method was used to melt the high-entropy alloy powder on the tantalum substrate to form a high-entropy alloy surface active layer. The laser power was 15kW and the scanning speed was 0.5mm s –1 , the overlap rate is 40%, and the cladding process is carried out under argon protection; the deposited high entropy alloy will produce a gradient grain structure with alternating growth of equiaxed crystals and columnar crystals due to cyclic heat input and rapid solidification; the surface active layer of the high entropy alloy after laser cladding is plasma treated and ceramicized to improve its surface activity and corrosion resistance. The plasma treatment uses a mixed gas of argon and oxygen, in which the volume fraction of oxygen is 10%, the processing power is 300w, the processing time is 20min, and the processing temperature is 50℃ to convert the high entropy alloy layer into a high entropy ceramic layer; a layer of nano titanium dioxide coating is prepared on the high entropy ceramic layer by a sol-gel method. First, butyl titanate, ethanol, acetylacetone and deionized water are mixed in a mass ratio of 8:2:10:1, stirred evenly to obtain a sol, and then the electrode is immersed in the sol at 4mm min –1 After repeated pulling and drying in air, heat treatment was carried out at a temperature of 450°C for 2 hours. Finally, the electrode was modified by ion doping technology to improve its electrocatalytic activity and selectivity. Molybdenum ions were selected for doping with a doping mass concentration of 3%. The doping method was electrochemical deposition with a deposition voltage of -1.0 V. The deposition process was carried out in an ammonium molybdate electrolyte with a mass concentration of 20%. The electrolyte temperature was 40°C. After the deposition time was 30 minutes, the electrode was taken out and washed with deionized water to obtain an ultra-stable high entropy metal oxide electrode that can be used for AC reversal.
[0036] Embodiment 2:
[0037] The anti-scaling performance of the ultrastable high entropy metal oxide electrode (hereinafter referred to as the sample electrode) obtained in Example 1 for AC reversal under different AC reversal conditions was tested. The test was carried out in a 150 mL glass container, with a sample electrode of 1 cm × 1 cm as the working electrode, a platinum sheet electrode as the counter electrode, and a saturated calomel electrode as the reference electrode. The reaction temperature was 60 ° C, and the CaCl2 concentration in the electrolyte was set to 300.0 mg L –1 , NaHCO3 concentration 300.0 mg L –1 , MgCl2 concentration is 150.0 mg L –1 , the supporting electrolyte Na2SO4 concentration is 1.0 g L–1 A periodic reversal current was applied to the sample electrode using a CHI660E electrochemical workstation with a current density of 10 mA cm –1 The inversion frequencies were 0 Hz (i.e. DC), 0.1 Hz, 10 Hz, and 20 Hz, respectively. After a certain reaction time, the sample electrode was subjected to in-situ measurements of AC impedance and linear scanning voltammetry. After the reaction was completed, the sample electrode was taken out and characterized by a scanning electron microscope.
[0038] At the same time, the initial CaCl2 concentration was adjusted to investigate the effect of different calcium ion concentrations on the scaling behavior of the sample electrode under 20Hz reversal conditions, mainly judging by the reduction of calcium ion concentration, and the calcium ion concentration was measured according to the national standard GB7476-1987. At pH 12-13, calcium ions were titrated using disodium EDTA solution.
[0039] Scanning electron microscope images are attached. Figure 1 As shown, with the gradual decrease of the reversal frequency, scaling becomes increasingly obvious, and even obvious larger crystals appear under DC conditions. Surface high-frequency (20Hz) AC reversal is beneficial to the active interface of the sample electrode.
[0040] Changes in exchange current intensity (Appendix Figure 2 ) also proved the above conclusion. Under the condition of 20Hz alternating current, a stable exchange current can be ensured on the surface of the sample electrode at all times, while under the condition of 0Hz, scaling is formed rapidly, causing the current to shrink rapidly to zero.
[0041] Under the conditions of AC reversal frequencies of 20Hz, 10Hz, 0.1Hz, and 0Hz, the AC impedance spectra of the sample electrodes are also very different. Under high-frequency conditions, the real ohmic value of the AC impedance is significantly lower than the ohmic value under low-frequency conditions (see Appendix Figure 3 ).
[0042] Under high frequency conditions, the effects of different calcium ion concentrations on the scaling behavior of the sample electrodes were investigated under 20 Hz reversal conditions. It was found that no significant scaling occurred on the sample electrodes within 60 min, the calcium ion concentration decreased slightly, and most of it was precipitated in the solution and not deposited on the electrode surface (attached Figure 4 ).
[0043] Embodiment 3:
[0044] The sample electrode prepared in the present invention and the commercially available lead oxide electrode were used to treat the landfill leachate collected from a landfill. The initial concentration (chemical oxygen demand) of the landfill leachate was 350 mg / L, and the hardness was 570 mg (CaCO3) / L. The electrocatalytic reactor was made of organic glass and had a volume of 30 (length) × 30 (width) × 50 (height) cm3 The working electrode is the sample electrode, with an area of 30 (length) × 30 (width) cm 2 , placed on one side of the reactor, and the counter electrode was a stainless steel plate of the same size as the working electrode, placed on the other side of the reactor. A square wave variable frequency power supply was used to provide an AC source with a current density of 10 mA cm -2 . Sampling was performed regularly, and the chemical oxygen demand concentration in the water samples was determined according to HJ 828-2017 (Water quality - Determination of chemical oxygen demand - potassium dichromate method).
[0045] The results showed that the commercially available lead oxide electrode could not maintain its catalytic activity under AC reversal conditions, and after 10 cycles of degradation testing, its activity loss exceeded 60% (see Appendix Figure 5 ); In contrast, the sample electrode can maintain a high electrocatalytic performance. After 10 cycles of testing, its activity has hardly changed significantly, and the degradation rate can be maintained above 95% for 300 min (see Appendix Figure 6 ).
[0046] Embodiment 4:
[0047] The sample electrode prepared in the present invention was used to treat the fracturing flowback fluid collected from a drilling site. The initial concentration (chemical oxygen demand) of the fracturing flowback fluid was 210 mg / L, and the hardness was 336 mg (CaCO3) / L. The results showed that the sample electrode can maintain a high electrocatalytic performance. After 10 cycles of testing, its activity showed almost no significant change, and the degradation rate for 300 minutes can be maintained at more than 80% (see Appendix). Figure 7 )
[0048] The specific implementation methods described above are only used to specifically illustrate the spirit of the present invention, and the protection scope of the present invention is not limited thereto. For those skilled in the art, other implementation methods can certainly be easily made by changing, replacing or modifying the technical contents disclosed in this specification, and these other implementation methods should all be included in the protection scope of the present invention.
Claims
1. An ultrastable high entropy metal oxide electrode that can be used for alternating current reversal, characterized in that: The preparation method of the electrode comprises the following steps: Step 1, the tantalum substrate is subjected to high-precision polishing treatment to make its surface roughness reach Ra 0.5μm, and then the polished tantalum substrate is placed in an ultrasonic cleaner, cleaned with acetone for 15 minutes to remove surface oil, then rinsed with deionized water, and then immersed in a dilute hydrochloric acid solution with a mass concentration of 5% for 15 minutes to remove surface oxides, and finally rinsed with deionized water and dried at a drying temperature of 100°C for 30 minutes; Step 2: Use ion implantation technology to form an ultra-stable anti-corrosion carbide layer. The implanted ions are titanium carbide ions and zirconium carbide ions. The implantation energy is 120 keV and the implantation dose is 8×10 16 ions cm -2 The injection process was carried out under a vacuum of 1×10 -3 The process was carried out in a Pa environment, with an injection temperature of 150°C and an injection time of 10 s to obtain a tantalum substrate with an ultra-stable anti-corrosion carbide layer; Step 3: Select 7 metal powders of tantalum, rubidium, gadolinium, dysprosium, chromium, nickel and cadmium according to the molar ratio of 120:7:16:22:9:2:1, and put the prepared raw materials into a planetary ball mill for mechanical alloying treatment at a speed of 400 rpm. -1 The ball-to-material ratio was 15:1, the ball milling time was 20 h, and argon protection was introduced during the ball milling process to prevent metal oxidation. The powder after ball milling was kept at a vacuum degree of 1×10 -2 Heat treatment was carried out in a vacuum environment of 1.5 Pa at a temperature of 800°C for 2 h to obtain a mixed powder of 7 metals; Step 4: Use argon as carrier gas to spray the mixed powder of the seven metals obtained in step 3 at a rate of 20 L min -1 The nozzle temperature was 1200°C, and the powder was sprayed line by line on the tantalum substrate with an ultra-stable anti-corrosion carbide layer obtained in step 2 after ion implantation. At the same time, the high-energy laser direct energy deposition method was used to melt the high-entropy alloy powder on the tantalum substrate to form a high-entropy alloy surface active layer. The laser power was 15 kW and the scanning speed was 0.5 mm s -1 The overlap rate is 40%, and the cladding process is carried out under argon protection; the deposited high entropy alloy will produce a gradient grain structure with alternating growth of equiaxed crystals and columnar crystals due to cyclic heat input and rapid solidification; Step 5, plasma treatment and ceramicization are performed on the surface active layer of the high entropy alloy after laser cladding obtained in step 4 to improve its surface activity and corrosion resistance. The plasma treatment uses a mixed gas of argon and oxygen, wherein the volume fraction of oxygen is 10%, the treatment power is 300w, the treatment time is 20min, and the treatment temperature is 50°C, so as to convert the high entropy alloy layer into a high entropy ceramic layer; Step 6, a nano titanium dioxide coating is prepared on the high entropy ceramic layer obtained in step 5 by a sol-gel method. First, butyl titanate, ethanol, acetylacetone and deionized water are mixed in a mass ratio of 8:2:10:1, stirred evenly to obtain a sol, and then the electrode is immersed in the sol at 4 mm min -1 Repeated pulling, drying in air and then heat treatment at 450°C for 2h; Step 7, finally, the electrode is modified by ion doping technology to improve its electrocatalytic activity and selectivity, molybdenum ions are selected for doping, the doping mass concentration is 3%, the doping method is electrochemical deposition, the deposition voltage is -1.0V, and the deposition process is carried out in an ammonium molybdate electrolyte containing a mass concentration of 20%. The electrolyte temperature is 40°C, and after the deposition time is 30 minutes, the electrode is taken out and washed with deionized water to obtain an ultra-stable high-entropy metal oxide electrode that can be used for AC reversal.
Citation Information
Patent Citations
High-risk wastewater treatment apparatus and treatment method for laboratory
CN104496094A
Boron doped diamond electrode and preparation method thereof
CN109750291A
Coated electrode for electrochemical water treatment electrode reversal and preparation method of coated electrode
CN116986684A
High-corrosion-resistance hydrogen evolution electrode material as well as preparation method and application thereof
CN118461047A
Electrode for electrolytic water treatment and apparatus using the same
JP2006322026A
Cited By
Method and device for producing medium-chain fatty acid through electric fermentation by using oxide high-entropy ceramic modified electrode