Method for ultrasonic oil removal of catholyte for electrolytic nickel production

Through ultrasonic oil removal and multi-layer oil removal processes, the problem of excessive oil content in the electrolytic nickel extraction residue is solved, the physical appearance and value of nickel electrolysis is improved, and the high-quality production of electrolytic nickel is achieved.

CN118993407AInactive Publication Date: 2024-11-22JILIN JIEN NICKEL INDUSTRY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411157831.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the electrolytic nickel production process, the oil content in the extraction residue is too high, which affects the surface smoothness and quality of the electrolytic nickel, leads to pore problems, and affects product value.

Method used

Ultrasonic oil removal method is adopted to remove oily substances on the surface through the oil separator tank, and the oil content in the liquid is reduced by using ultrasonic demulsification and constant flow chamber, gas vibration chamber, release chamber and other equipment. The liquid is adjusted by combining desulfurization and multi-layer oil removal processes. The pH value and oil content reach a reasonable range.

Benefits of technology

It effectively reduces the oil content of the cathode liquid, improves the physical appearance and value of electrolytic nickel, and ensures the high quality and market competitiveness of the product.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a method for ultrasonic oil removal of a catholyte for electrolytic nickel production, and belongs to the technical field of hydrometallurgy, oil-removed extraction raffinate is used as the catholyte, and the oil removal process of the catholyte comprises the steps of surface oily substance removal through an oil separation tank, ultrasonic first-stage oil removal, desulfurization, ultrasonic second-stage oil removal and the like. The oil content of the catholyte for preparing the electrolytic nickel is controlled to the minimum, so that the appearance of the electrolytic nickel can be improved, the growth of the electrolytic nickel is prevented from being adhered by oily ions in the catholyte, the uniform distribution of power lines is ensured, and the revenue profit of an enterprise is increased on the basis of not increasing the labor cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrometallurgy, and particularly relates to a method for ultrasonically degreasing cathode liquid used in electrolytic nickel production. Technical Background

[0002] The process of directly casting high-grade nickel matte into anode plates to produce electrolytic nickel is the process adopted by major domestic electrolytic nickel manufacturers. In order to ensure that the cathode liquid index is qualified, an extraction process is set up. Since a large amount of kerosene and extractant need to be added in the extraction process, some oil will be mixed in the liquid during the separation process. When the cathode liquid contains too much oil, pores will appear on the surface of the electrolytic nickel during the later growth process.

[0003] In summary, in order to solve the impact of excessive oil content in the liquid on the quality of electrolytic nickel, improve the surface smoothness of electrolytic nickel, and increase sales profits, our company specially proposes a production method for ultrasonic degreasing to improve the quality of electrolytic nickel. Summary of the invention

[0004] The technical problem to be solved by the present invention is to reduce the oil content in the extraction residual liquid and bring the oil content in the liquid into a reasonable range.

[0005] A method for ultrasonically degreasing cathode liquid for electrolytic nickel production, using the degreasing residual liquid as cathode liquid, and the degreasing process of the cathode liquid comprises the following steps:

[0006] Step 1: Take 272 extraction residual liquid with a pH value between 4.8-5, and let the liquid flow into the oil separator to remove the surface oily substances;

[0007] Step 2: After the oily substances on the surface are removed from the oil separator, the liquid is pumped into the ultrasonic first stage for oil removal;

[0008] Step 3: Pump the liquid into the desulfurization process for chlorine desulfurization, and adjust the liquid pH to between 4.8-5.3;

[0009] Step 4: The liquid after the desulfurization process is pumped into the ultrasonic second-stage oil removal, and then the oil is removed by adsorption to obtain the cathode liquid suitable for nickel electrolysis.

[0010] Preferably, in step 1, the oil removal tanks are interconnected to continuously demulsify, float, filter and remove the oily substances that are difficult to separate from the liquid, and finally obtain a cathode liquid with a lower oil content.

[0011] Preferably, a constant flow chamber, an air vibration chamber and a release chamber are respectively provided for ultrasonic first-stage oil removal and ultrasonic second-stage oil removal. The liquid passes through the constant flow chamber to remove solid impurities on the surface of the liquid and then enters the air vibration chamber. The liquid is demulsified by ultrasonic air vibration and the floating oil floats to the surface.

[0012] Preferably, after demulsification, the liquid is pumped into a buffer tank in the buffer chamber, the oily substance is salvaged out of the system, and the liquid flows from the buffer tank into a lifting tank.

[0013] Preferably, the liquid after the first-stage oil removal in step 2 is pumped into the grinding and leaching workshop through a first-stage lifting tank for desulfurization process.

[0014] Preferably, after the second stage of oil removal, the liquid is again subjected to fiber ball column oil removal and activated carbon column oil removal, and the final liquid oil content index is between 0.1-0.13, thereby obtaining a cathode liquid suitable for nickel electrolysis.

[0015] Through the above-mentioned design scheme, the present invention can bring the following beneficial effects: reducing the oil content of the cathode liquid used in electrolytic nickel and improving the physical appearance of electrolytic nickel. Since the physical appearance of electrolytic nickel directly depends on the price, this scheme actually directly improves the value of electrolytic nickel. DETAILED DESCRIPTION

[0016] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention, and matters not described in the present invention are applicable to the prior art.

[0017] Example 1

[0018] A method for ultrasonically degreasing cathode liquid for electrolytic nickel production, using the degreasing residual liquid as cathode liquid, and the degreasing process of the cathode liquid comprises the following steps:

[0019] Step 1: Take 272 extraction residual liquid with a pH value of 4.8, copper content <0.002g / L and oil content index of 15, and the liquid flows into the oil separator to remove the oily substances on the surface. In the above steps, the oil removal tanks are interconnected to continuously demulsify, float, filter and remove the oily substances that are difficult to separate in the liquid, and finally obtain a cathode liquid with a lower oil content.

[0020] Step 2: After the oily substances on the surface are removed in the oil separator, the liquid is pumped into the ultrasonic first-stage oil removal (80t);

[0021] The first stage of ultrasonic oil removal is equipped with a constant flow chamber, an air vibration chamber, a release chamber and a lifting chamber. The liquid passes through the constant flow chamber to remove solid impurities on the liquid surface and then enters the air vibration chamber. The liquid is demulsified by ultrasonic air vibration, and the floating oil floats to the surface. After demulsification, the liquid is pumped into the buffer tank, and the oily substances are salvaged out of the system. The liquid flows into the first stage lifting pool, and the oil content index is reduced to 0.35.

[0022] Step 3: The liquid after degreasing is pumped into the grinding and leaching workshop through a lifting tank for desulfurization process, and the pH of the liquid is adjusted to about 5.2.

[0023] Step 4: The liquid after the desulfurization process is pumped into the ultrasonic two-stage oil removal (80t). The liquid passes through the constant flow chamber, gas vibration chamber, release chamber and lifting chamber, and the final liquid oil content index is about 0.2. It then enters the fiber ball deoiler and activated carbon deoiler, and the final cathode liquid oil content index reaches 0.12.

[0024] Example 2

[0025] A method for ultrasonically degreasing cathode liquid for electrolytic nickel production, using the degreasing residual liquid as cathode liquid, and the degreasing process of the cathode liquid comprises the following steps:

[0026] Step 1: Take 272 extraction residual liquid with a pH value of 4.9, copper content <0.002g / L and oil content index of 10, and the liquid flows into the oil separator to remove the oily substances on the surface. In the above steps, the oil removal tanks are interconnected to continuously demulsify, float, filter and remove the oily substances that are difficult to separate in the liquid, and finally obtain a cathode liquid with a lower oil content.

[0027] Step 2: After the oily substances on the surface are removed from the oil separator, the liquid is pumped into the ultrasonic first stage for oil removal;

[0028] The first stage of ultrasonic oil removal is equipped with a constant flow chamber, an air vibration chamber, a release chamber and a lifting chamber. The liquid passes through the constant flow chamber to remove solid impurities on the liquid surface and then enters the air vibration chamber. The liquid is demulsified by ultrasonic air vibration, and the floating oil floats to the surface. After demulsification, the liquid is pumped into the buffer tank, and the oily substances are salvaged out of the system. The liquid flows from the buffer tank into the first stage lifting tank, and the oil content index is reduced to 0.2.

[0029] Step 3: The liquid after degreasing is pumped into the grinding and leaching workshop through a lifting tank for desulfurization process, and the pH of the liquid is adjusted to about 5.3.

[0030] Step 4: The liquid after the desulfurization process is pumped into the ultrasonic second-stage oil removal. The ultrasonic second-stage oil removal is also equipped with a constant flow chamber, an air vibration chamber, a release chamber and a lifting chamber. The liquid passes through the constant flow chamber, the air vibration chamber, the release chamber and the lifting chamber again, and then enters the fiber ball deoiler and the activated carbon deoiler. Finally, the cathode liquid oil content index reaches 0.1.

[0031] Example 3

[0032] A method for ultrasonically degreasing cathode liquid for electrolytic nickel production, using the degreasing residual liquid as cathode liquid, and the degreasing process of the cathode liquid comprises the following steps:

[0033] Step 1: Take 272 extraction residual liquid with a pH value of 5.0, copper content <0.002g / L and oil content index of 18. The above liquid flows into the oil separator to remove the oily substances on the surface. In the above steps, the oil removal tanks are interconnected to continuously demulsify, float and filter the oily substances that are difficult to separate in the liquid to finally obtain a cathode liquid with a lower oil content.

[0034] Step 2: After the oily substances on the surface are removed from the oil separator, the liquid is pumped into a degreasing section;

[0035] The first stage of oil removal is equipped with a constant flow chamber, an air vibration chamber, a release chamber and a lifting chamber. The liquid passes through the constant flow chamber to remove solid impurities on the liquid surface and then enters the air vibration chamber. The liquid is demulsified by ultrasonic air vibration, and the floating oil floats to the surface. After demulsification, the liquid is pumped into the buffer tank, and the oily substances are salvaged out of the system. The liquid flows from the buffer tank into the first stage lifting pool, and the oil content index is reduced to 0.22.

[0036] Step 3: The liquid after degreasing is pumped into the grinding and leaching workshop through a lifting tank for desulfurization process, and the pH of the liquid is adjusted to about 4.8.

[0037] Step 4: The liquid after the desulfurization process is pumped into the second stage of oil removal. The second stage of oil removal is also equipped with a constant flow chamber, an air vibration chamber, a release chamber and a lifting chamber. The liquid passes through the constant flow chamber, the air vibration chamber, the release chamber and the lifting chamber again, and then enters the fiber ball deoiler and the activated carbon deoiler. Finally, the oil content index of the cathode liquid reaches 0.12.

Claims

1. A method for ultrasonic degreasing of cathode liquid for electrolytic nickel production, characterized in that: The deoiled extraction raffinate is used as the cathode liquid, and the deoiling process of the cathode liquid includes the following steps: Step 1: Take 272 extraction residual liquid with a pH value between 4.8-5, and let the liquid flow into the oil separator to remove the surface oily substances; Step 2: After the oily substances on the surface are removed from the oil separator, the liquid is pumped into the ultrasonic first stage for oil removal; Step 3: Pump the liquid into the desulfurization process for chlorine desulfurization, and adjust the liquid pH to between 4.8-5.3; Step 4: The liquid after the desulfurization process is pumped into the ultrasonic second-stage oil removal, and then the oil is removed by adsorption to obtain the cathode liquid suitable for nickel electrolysis.

2. The method for improving the quality of electrolytic nickel by ultrasonic gas vibration degreasing according to claim 1, characterized in that: In step 1, the oil removal tanks are interconnected to continuously demulsify, float, filter and remove the oily substances that are difficult to separate in the liquid, and finally obtain a cathode liquid with a low oil content.

3. The method for improving the quality of electrolytic nickel by ultrasonic gas vibration degreasing according to claim 1, characterized in that: The ultrasonic first-stage oil removal and ultrasonic second-stage oil removal are respectively provided with a constant flow chamber, an air vibration chamber, a release chamber and a lifting chamber. The liquid passes through the constant flow chamber to remove solid impurities on the surface of the liquid and then enters the air vibration chamber. The liquid is demulsified by ultrasonic air vibration and the floating oil floats to the surface.

4. The method for improving the quality of electrolytic nickel by ultrasonic gas vibration degreasing according to claim 1, characterized in that: After demulsification, the liquid is pumped into the buffer tank of the release chamber, the oily matter is salvaged out of the system, and the liquid flows into a lifting tank.

5. The method for improving the quality of electrolytic nickel by ultrasonic gas vibration degreasing according to claim 1, characterized in that: The liquid after the first stage of oil removal in step 2 is pumped into the grinding and leaching workshop through a lifting tank for desulfurization process.

6. The method for improving the quality of electrolytic nickel by ultrasonic gas vibration degreasing according to claim 1, characterized in that: After the second stage of degreasing, the liquid is again degreasing by fiber ball column and activated carbon column, and the final liquid oil content index is between 0.1-0.15, thereby obtaining a cathode liquid suitable for electrolytic nickel.

Citation Information

Patent Citations

  • Preparation method for reducing sulfur impurities in electrolytic nickel

    CN103498169A

  • Oil removal system and method for high-concentration oily sewage

    CN114477576A

  • Method of eliminating oil from nickel chloride solution

    CN1924041A

  • Integration ultrasonic deoiler

    CN202542983U

  • Ultrasonic demulsification coalescence air flotation oil removal combined device

    CN214936709U