System and method for capturing and mineralizing converter flue gas CO2 through steel slag-wastewater
Through the Ca2+ leaching reaction of steel slag powder and cold-rolled wastewater and the three-phase mineralization of converter flue gas, mineralized steel slag is generated and mixed with cement clinker, the problem of difficult use of steel slag, wastewater and flue gas is solved, and low-carbon Cement production and carbon emissions in the steel industry are reduced.
Patent Information
- Application Number
- CN202411000248.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-22
AI Technical Summary
It is difficult to use steel slag, cold-rolled wastewater and steel plant flue gas to resource utilization or effectively dispose of, resulting in high carbon emissions and wastewater treatment costs in the steel industry.
The Ca2+ leaching reaction is carried out with the micro-slag powder and cold-rolled wastewater, and then the gas-liquid-solid three-phase mineralization reaction is carried out with the converter flue gas to generate mineralized steel slag, and mixed with cement clinker to prepare low-carbon green cement, and recycle it. The filtrate reduces the difficulty of wastewater treatment.
The conversion rate of activated calcium oxide and magnesium in steel slag is improved, the CO2 reaction efficiency is enhanced, carbon emissions and wastewater treatment costs are reduced, and the coordinated treatment of steel slag, wastewater and flue gas and the production of low-carbon cement are realized.
Smart Images

Figure CN118993582A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of energy conservation and environmental protection, and in particular to a system and method for capturing CO2 from mineralized converter flue gas using steel slag and wastewater. Background Art
[0002] The statements in this section merely provide background information related to the present disclosure and may not constitute prior art.
[0003] The steel industry is one of the main sources of carbon emissions in domestic industry. Steel slag is the main waste slag produced in the steelmaking process. In 2020, the national steel slag production reached 160 million tons, but its comprehensive utilization rate was only 30%. There is an urgent need for steel slag stabilization and resource processing technology. The steel park emits a large amount of flue gas CO2 gas every year. Steel slag contains substances such as dicalcium silicate, f-CaO, and f-MgO. The steel slag mineralization technology can convert active calcium oxide and other substances into stable calcium carbonate, which can achieve the coordinated management of solid waste and carbon emission reduction. At the same time, the high-calcium content wastewater (such as cold rolling wastewater) generated by the steelmaking process currently needs to be treated with a complete set of pretreatment processes such as calcium and magnesium removal. In the steel slag mineralization technology, the use of such cold rolling wastewater as a medium for wet mineralization can not only reduce the demand for water resources, but also the salt in the steel plant wastewater can strengthen the mineralization process and improve the mineralization capacity of steel slag. At the same time, after a certain amount of pollutants such as calcium ions, alkalinity and salt substances are consumed in the wastewater, it is conducive to reducing the difficulty and cost of subsequent wastewater treatment.
[0004] Using high-calcium wastewater generated by the steelmaking process, such as cold rolling wastewater, steel slag combined with steel plant wastewater mineralization to capture converter flue gas can achieve the coordinated disposal of CO2 capture, steel slag resource utilization, and low-cost green treatment of steel plant wastewater, providing technical support for the industrial application of steel slag mineralization technology. Patent 201911352090.X discloses a method for preparing high-purity nano-calcium carbonate using steel slag, converter flue gas and steel plant wastewater. The advantage of this method is that the waste gas, waste liquid and waste slag generated by the steelmaking process are used at the same time to prepare nano-scale calcium carbonate, but the performance of the steel slag leached by this process is not completely stable, and the document does not consider the subsequent treatment of the leached steel slag, which cannot achieve resource utilization or effective disposal. Therefore, exploring the use of steel slag mixed with steel plant wastewater mineralization to capture steel plant flue gas CO2 and realize the economical and effective coordinated treatment of the three wastes in the steel industry is of great significance to the steel production process. Summary of the invention
[0005] The purpose of the present invention is to provide a system and method for capturing mineralized converter flue gas CO2 using steel slag-wastewater in response to the problem that steel slag, cold rolling wastewater and steel mill flue gas CO2 are currently difficult to realize resource utilization or effective disposal, thereby achieving coordinated treatment of steel slag, wastewater and converter flue gas in steel plants, reducing carbon emissions in the steel industry's production process and subsequent treatment costs of steel plant wastewater, and preparing green and low-carbon cement building materials.
[0006] The technical solution of the present invention is as follows:
[0007] A method for capturing CO2 from mineralized converter flue gas using steel slag-wastewater, comprising the following steps:
[0008] (1) crushing and grinding the steel slag into steel slag powder, preferably steel slag powder less than 150 microns to participate in subsequent reactions;
[0009] (2) Place steel slag powder and steel mill wastewater in a mixing device and stir them to obtain Ca 2+ Leaching reaction, the liquid-to-solid ratio of the steel plant wastewater and the steel slag powder is 10-50mL:1g, the reaction time is 20-60min, and the leached Ca is obtained after the reaction. 2+ Mixed steel slag slurry;
[0010] The preferred liquid-to-solid ratio of steel mill wastewater and steel slag powder is 20-40 mL:1 g, and the mixing reaction time is 20-30 min.
[0011] (3) The leached Ca is pumped 2+ The mixed steel slag slurry is transported to the mineralization reactor, and the converter flue gas at 50-70°C is introduced to carry out a gas-liquid-solid three-phase mineralization reaction. The mineralization reaction time is 60-120 minutes.
[0012] Preferably, the mineralization reaction time is 60 to 90 minutes. Preferably, the converter flue gas in step (3) is preferably 20% to 30% CO2 converter flue gas by volume.
[0013] (4) separating the solid and liquid of the mineralized slurry after the reaction to obtain mineralized steel slag and filtrate, and returning the filtrate to step (2) for recycling as a leaching solution;
[0014] Preferably, the method further comprises step (5) of mixing and grinding the mineralized steel slag and cement clinker to obtain low-carbon green cement, wherein the mixing ratio is cement clinker: mineralized steel slag = 80-90: 20-10, and the strength of the cement is increased by 5-10% after mixing.
[0015] According to a preferred embodiment, the preferred steel slag in step (1) is converter steel slag, wherein the CaO content is about 30% to 40%, the MgO content is about 5% to 13%, the SiO2 content is about 20% to 25%, the Al2O3 content is about 15% to 20%, and the Fe2O3 content is about 10% to 15%.
[0016] According to a preferred embodiment, the steel mill wastewater in step (2) is preferably cold rolling wastewater, and its components include Ca 2+ :200~300mg / L、Mg 2+ : 40~100mg / L, and its pH is 12~14.
[0017] According to a preferred embodiment, the mineralization reactor in step (3) is equipped with a stirring device, and the stirring rate is 80 to 120 rpm, preferably 100 to 120 rpm.
[0018] According to a preferred embodiment, in step (3), the mixed steel slag slurry is pumped into the mineralization reactor from the top, and the converter flue gas is added from the bottom of the mineralization reactor, and the volume flow ratio of the mixed steel slag slurry to the converter flue gas is 1:30 to 50; preferably 1:30 to 40.
[0019] According to a preferred embodiment, in step (4), the mineralized steel slag slurry is filtered and separated to obtain mineralized steel slag and filtrate, and the mineralized steel slag is mixed with cement clinker to obtain low-carbon cement, and the filtrate can be recycled to step (2) at a recycling ratio of 30% to 50%, and the remaining filtrate is transported to the steel plant wastewater network. The preferred recycling ratio is 40% to 50%.
[0020] Another aspect of the present invention provides a system for capturing CO2 from mineralized converter flue gas using steel slag-wastewater, comprising a pulverizer, a leaching device, a mineralization reactor and a filter;
[0021] The steel slag powder crushed by the crusher is transported to the leaching device, and cold rolling wastewater is introduced into the leaching device at the same time, so that the cold rolling wastewater and the steel slag powder are mixed and reacted in the leaching device to generate mixed steel slag slurry;
[0022] The mixed steel slag slurry after the reaction is fed into the mineralization reactor from the top, and the converter flue gas is introduced from the bottom of the mineralization reactor. The speed of the agitator inside the mineralization reactor is controlled, and a three-phase mineralization reaction of steel slag, cold rolling wastewater and converter flue gas is carried out in the mineralization reactor to obtain mineralized steel slag.
[0023] The products after the three-phase mineralization reaction are filtered and separated in a filter to obtain mineralized steel slag and filtrate. The obtained mineralized steel slag can be used as a raw material product for downstream utilization, and part of the filtrate is transported back to the leaching device for recycling.
[0024] Preferably, a mixer is also included, and the obtained mineralized steel slag is transported to the mixer to be mixed with cement clinker and ground into powder to prepare low-carbon green cement.
[0025] Preferably, the system further comprises a slurry delivery pump and a filtrate delivery pump, and the mixed steel slag slurry after the reaction is delivered from the top of the mineralization reactor by the slurry delivery pump;
[0026] The products after the three-phase mineralization reaction are filtered and separated in a filter to obtain mineralized steel slag and filtrate. The obtained mineralized steel slag can be used as a raw material product for downstream utilization, and part of the filtrate is transported back to the leaching device for recycling through a filtrate delivery pump.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1. A system and method for capturing CO2 from converter flue gas by using slag-wastewater for mineralization. The present application adopts a three-phase mineralization method. Compared with the two-phase mineralization reaction, the slag raw material directly participates in the reaction system in the three-phase reaction, which can increase the conversion rate of active calcium oxide and magnesium in the slag. At the same time, mechanical stirring increases the mass transfer rate between the slag slurry and the converter flue gas, thereby improving the slag mineralization carbon fixation rate.
[0029] 2. A system and method for capturing and mineralizing converter flue gas CO2 with steel slag and wastewater. The reaction efficiency between steel slag and carbon dioxide in converter flue gas is significantly improved through premixing, gas-liquid-solid three-phase mass transfer reaction and other process means. Under the optimal process conditions, the carbon fixation rate of steel slag can reach 10%, and the mineralization rate of steel slag can reach 65%. The alkalinity and Ca in the wastewater of the steel plant are reduced. 2+ The substances are fully utilized in the synergistic mineralization process, which effectively reduces the difficulty and cost of subsequent wastewater treatment;
[0030] 3. A system and method for capturing CO2 from converter flue gas by using steel slag and wastewater to mineralize the converter flue gas. The present invention proposes a system and method for producing low-carbon cement by using steel slag, wastewater and carbon dioxide captured from converter flue gas to undergo mineralization reaction. Cold rolling wastewater from the steel plant is mixed with steel slag to form a slurry, which strengthens the leaching effect of calcium ions in the steel slag and improves the mineralization efficiency of the steel slag. The converter flue gas is reacted with the slurry to form mineralized steel slag, which is then mixed with ordinary cement to prepare low-carbon cement. The implementation of the present invention achieves the coordinated management of steel slag, wastewater and converter flue gas in steel plants, reduces carbon emissions in the steel industry production process and the subsequent treatment costs of steel plant wastewater, and prepares green low-carbon cement building materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a schematic diagram of the system flow of using steel slag-wastewater to capture CO2 from mineralized converter flue gas.
[0032] Figure numerals: 1-crusher, 2-leaching device, 3-mineralization reactor, 4-filter, 5-mixer, 6-slurry delivery pump, 7-filtrate delivery pump. DETAILED DESCRIPTION
[0033] The specific embodiments listed in the present invention are only examples of the present invention, and the present invention is not limited to the specific embodiments described below. For those skilled in the art, any equivalent modifications and substitutions to the embodiments described below are also within the scope of the present invention. Therefore, the equal transformations and modifications made without departing from the spirit and scope of the present invention should be included in the scope of the present invention. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturers are not specified for all reagents or instruments, they are all conventional products that can be purchased commercially. In order to better illustrate the present invention, numerous specific details are given in the specific embodiments below. It should be understood by those skilled in the art that the present invention can also be implemented without certain specific details. In other embodiments, the methods, means, equipment and steps well known to those skilled in the art are not described in detail in order to highlight the purport of the present invention.
[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art. Unless otherwise specified, the units used in this specification are all international standard units, and the numerical values and numerical ranges appearing in the present invention should be understood to include the inevitable systematic errors in industrial production.
[0035] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0036] The exemplary composition of the steel slag used in the embodiment of the present invention includes 35% CaO, 6% MgO, 24% SiO2, 17% Al2O3, and 12% Fe2O3 by mass percentage.
[0037] The ion concentrations of the cold rolling wastewater used in the embodiment of the present invention are: Ca 2+ :260mg / L、Mg 2+ : 50 mg / L, and its pH is 12.
[0038] The converter flue gas used in the embodiment of the present invention contains 28% CO2 by volume.
[0039] Example 1
[0040] See also Figure 1 , a system and method for capturing CO2 from mineralized converter flue gas using steel slag-wastewater,
[0041] (1) The pulverizer 1 crushes the steel slag to obtain steel slag powder of less than 150 microns, which participates in the subsequent reaction;
[0042] (2) The steel slag powder and cold rolling wastewater obtained by pulverizing in step (1) are transported to the leaching device 2 for mixing. The ratio of cold rolling wastewater to steel slag powder is controlled to be 20 mL:1 g, and the mixing reaction time is 20 min.
[0043] (3) After step (1), the slag slurry is delivered from the top of the mineralization reactor 3 using the slurry delivery pump 6, and the converter flue gas is introduced from the bottom of the mineralization reactor 3. The volume flow ratio of the slag slurry to the converter flue gas is controlled to be approximately 1:30, the agitator speed is controlled to be 80 rpm, and the reaction time of the slag slurry is controlled to be 60 min.
[0044] (4) After step (2), the mineralized steel slag slurry is separated by filter 4 to obtain mineralized steel slag and filtrate. The mineralized steel slag is used as a raw material product for downstream utilization. 30% of the filtrate is returned to step (1) for recycling through the filtrate delivery pump 7, and the remaining filtrate is discharged into the steel slag wastewater tank.
[0045] (5) The mineralized steel slag is filtered and mixed with cement clinker to prepare low-carbon green cement through a mixer 5. The mixing mass ratio of the mineralized steel slag to the cement clinker is 20:80. After mixing, the cement strength is increased by 5.4%.
[0046] The carbon fixation rate of steel slag reaches 5%, and the mineralization rate of steel slag, that is, the conversion rate of active calcium oxide and magnesium in steel slag, reaches 42%.
[0047] Example 2
[0048] See also Figure 1 , a system and method for capturing CO2 from mineralized converter flue gas using steel slag-wastewater,
[0049] (1) The pulverizer 1 crushes the steel slag to obtain steel slag powder of less than 150 microns, which participates in the subsequent reaction;
[0050] (2) The steel slag powder with a size less than 150 μm obtained by crushing in the pulverizer 1 and the alkaline steel plant wastewater are transported to the leaching device 2 for mixing, the liquid-to-solid ratio is controlled to be 30 mL:1 g, and the mixing reaction time is 30 min.
[0051] (3) After step (1), the slurry delivery pump 6 is used to deliver the steel slag slurry from the top of the mineralization reactor 3, and the converter flue gas is introduced from the bottom of the mineralization reactor 3. The volume flow ratio of the steel slag slurry to the converter flue gas is controlled to be approximately 1:30, the agitator speed is controlled to be 90 rpm, and the reaction time of the steel slag slurry is controlled to be 75 min.
[0052] (4) After step (2), the mineralized steel slag slurry is separated by filter 4 to obtain mineralized steel slag and filtrate. The mineralized steel slag is used as a raw material product for downstream utilization, and 50% of the filtrate is returned to step (1) for recycling through the filtrate delivery pump 7. The remaining filtrate is discharged into the steel slag wastewater tank.
[0053] (5) The mineralized steel slag is filtered and mixed with cement clinker to prepare low-carbon green cement through a mixer 5. The mixing mass ratio of the mineralized steel slag to the cement clinker is 20:80. After mixing, the cement strength is increased by 6.2%.
[0054] The carbon fixation rate of steel slag reaches 6%, and the mineralization rate of steel slag reaches 47%.
[0055] Example 3
[0056] See also Figure 1 , a system and method for capturing CO2 from mineralized converter flue gas using steel slag-wastewater,
[0057] (1) The pulverizer 1 crushes the steel slag to obtain steel slag powder of less than 150 microns, which participates in the subsequent reaction;
[0058] (2) The steel slag powder with a size less than 150 μm obtained by crushing in the pulverizer 1 and the alkaline steel plant wastewater are transported to the leaching device 2 for mixing, the liquid-to-solid ratio is controlled to be 40 mL:1 g, and the mixing reaction time is 40 min.
[0059] (3) After step (1), the slag slurry is delivered from the top of the mineralization reactor 3 using the slurry delivery pump 6, and the converter flue gas is introduced from the bottom of the mineralization reactor 3. The volume flow ratio of the slag slurry to the converter flue gas is controlled to be approximately 1:40, the agitator speed is controlled to be 100 rpm, and the reaction time of the slag slurry is controlled to be 90 min.
[0060] (4) After step (2), the mineralized steel slag slurry is separated by filter 4 to obtain mineralized steel slag and filtrate. The mineralized steel slag is used as a raw material product for downstream utilization, and 40% of the filtrate is returned to step (1) for recycling through the filtrate delivery pump 7. The remaining filtrate is discharged into the steel slag wastewater tank.
[0061] (5) The mineralized steel slag is filtered and mixed with cement clinker to prepare low-carbon green cement through a mixer 5. The mixing mass ratio of the mineralized steel slag to the cement clinker is 15:85. After mixing, the cement strength is increased by 7.8%.
[0062] The carbon fixation rate of steel slag reaches 8%, and the mineralization rate of steel slag reaches 55%.
[0063] Example 4
[0064] See also Figure 1 , a system and method for capturing CO2 from mineralized converter flue gas using steel slag-wastewater,
[0065] (1) The pulverizer 1 crushes the steel slag to obtain steel slag powder of less than 150 microns, which participates in the subsequent reaction;
[0066] (2) The steel slag powder with a size of less than 150 μm obtained by crushing in the pulverizer 1 and the alkaline steel plant wastewater are transported to the leaching device 2 for mixing, the liquid-to-solid ratio is controlled to be 50 mL:1 g, and the mixing reaction time is 60 min.
[0067] (3) After step (1), the slag slurry is delivered from the top of the mineralization reactor 3 using the slurry delivery pump 6, and the converter flue gas is introduced from the bottom of the mineralization reactor 3. The volume flow ratio of the slag slurry to the converter flue gas is controlled to be approximately 1:50, the agitator speed is controlled to be 120 rpm, and the reaction time of the slag slurry is controlled to be 120 min.
[0068] (4) After step (2), the mineralized steel slag slurry is separated by filter 4 to obtain mineralized steel slag and filtrate. The mineralized steel slag is used as a raw material product for downstream utilization, and 50% of the filtrate is returned to step (1) for recycling through the filtrate delivery pump 7. The remaining filtrate is discharged into the steel slag wastewater tank.
[0069] (5) The mineralized steel slag is filtered and mixed with cement clinker to prepare low-carbon green cement through a mixer 5. The mixing mass ratio of the mineralized steel slag to the cement clinker is 10:90. After mixing, the cement strength is increased by 9.8%.
[0070] The carbon fixation rate of steel slag reaches 10%, and the mineralization rate of steel slag reaches 65%.
[0071] Comparative Example 1
[0072] See also Figure 1 , a system and method for capturing CO2 from mineralized converter flue gas using steel slag-wastewater,
[0073] According to the test parameters of Example 4 of the present application, after the leachate is separated from the slag in step (3), the leachate is sent to the mineralization reactor 3, and the leachate and the converter flue gas are used for mineralization, and the active calcium oxide and magnesium conversion rate in the slag and the slag carbon fixation rate are obtained to be 5%, and the mineralization rate of the slag is 40%; the separated slag has unstable performance and cannot be mixed with cement clinker to prepare low-carbon cement.
[0074] The above-mentioned embodiments only express the specific implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the protection scope of the present application. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the technical solution concept of the present application, and these all belong to the protection scope of the present application.
Claims
1. A method for capturing CO2 from mineralized converter flue gas using steel slag-wastewater, characterized in that: The steps include: Step (1): crushing and grinding the steel slag into steel slag powder of less than 150 μm for subsequent reactions; Step (2): The steel slag powder prepared in step (1) and the steel mill wastewater are placed in a mixing device and stirred for Ca 2+ Leaching reaction, the liquid-to-solid ratio of the steel plant wastewater and the steel slag powder is 10-50mL:1g, the reaction time is 20-60min, and the leached Ca is obtained after the reaction. 2+ Mixed steel slag slurry; Step (3): Leaching Ca 2+ The mixed steel slag slurry is transported to the mineralization reactor, and the converter flue gas is introduced to carry out gas-liquid-solid three-phase mineralization reaction. The mineralization reaction time is 60 to 120 minutes. Step (4): After the reaction is completed, the mineralized slurry is separated into solid and liquid to obtain mineralized steel slag and filtrate.
2. The method for capturing CO2 from mineralized converter flue gas using steel slag-wastewater according to claim 1, characterized in that: In step (3), the volume flow ratio of converter flue gas to mixed steel slag slurry is 1:30-50.
3. The method for capturing CO2 from mineralized converter flue gas using steel slag-wastewater according to claim 2, characterized in that: In step (3), the volume flow ratio of converter flue gas to mixed steel slag slurry is 1:30-40.
4. The method for capturing CO2 from mineralized converter flue gas using steel slag-wastewater according to claim 1, characterized in that: In step (2), the liquid-to-solid ratio of the steel mill wastewater and the steel slag powder is 20-40 mL:1 g, and the mixing reaction time is 20-30 min.
5. The method for capturing CO2 from mineralized converter flue gas using steel slag-wastewater according to claim 1, characterized in that: The mineralization reaction time in step (3) is 60 to 90 minutes.
6. The method for capturing CO2 from mineralized converter flue gas using steel slag-wastewater according to claim 1, characterized in that: The filtrate in step (4) is returned to step (2) for recycling as leaching solution, with the return ratio being 30% to 50%.
7. The method for capturing CO2 from mineralized converter flue gas by using steel slag and wastewater according to claim 1, characterized in that: The method further comprises step (5): low-carbon green cement can be prepared by mixing and grinding the mineralized steel slag and cement clinker, wherein the mixing ratio is cement clinker: mineralized steel slag = 80-90: 20-10.
8. The method for capturing CO2 from mineralized converter flue gas using steel slag-wastewater according to claim 1, characterized in that: The steel mill wastewater in step (2) is cold rolling wastewater, and its components include Ca 2+ :200~300mg / L、Mg 2+ : 40~100mg / L, and its pH is 12~14.
9. The method for capturing CO2 from mineralized converter flue gas by using steel slag and wastewater according to claim 1, characterized in that: The converter flue gas described in step (3) is a CO2 converter flue gas with a temperature of 50-70°C and a volume percentage of 20%-30%.
10. A system for capturing CO2 from mineralized converter flue gas using steel slag and wastewater, characterized in that: The method comprises a pulverizer (1), a leaching device (2), a mineralization reactor (3) and a filter (4); The steel slag powder crushed by the crusher is transported to the leaching device (2), and cold rolling wastewater is introduced into the leaching device (2) at the same time, so that the cold rolling wastewater and the steel slag powder are mixed and reacted in the leaching device (2) to generate mixed steel slag slurry; The mixed steel slag slurry after the reaction is fed into the mineralization reactor (3) from the top, and the converter flue gas is introduced from the bottom of the mineralization reactor (3). The speed of the stirrer of the mineralization reactor (3) is controlled, and a three-phase mineralization reaction of the steel slag, cold rolling wastewater and converter flue gas is carried out in the mineralization reactor (3) to obtain mineralized steel slag; The product after the three-phase mineralization reaction is filtered and separated in a filter (4) to obtain mineralized steel slag and filtrate. The obtained mineralized steel slag can be used as a raw material product for downstream utilization, and part of the filtrate is transported back to the leaching device (2) for recycling.
Citation Information
Patent Citations
Method for capturing carbon dioxide and coproducing NPCC in converter flue gas by converter steel slag-steelmaking wastewater closed cycle
CN110950338A
Cited By
Cooperative method and system for capturing and mineralizing and fixing CO2 in steel slag treatment tail gas
CN121060267A