Mud-resistant concrete water reducing agent and preparation method thereof
By using mud-resistant concrete water reducer in concrete, combined with polycarboxylic acid water reducer, quaternized silicone and bentonite, the problem of deterioration in concrete performance caused by high sand mud content is solved, and the resistance of concrete is improved Pressure and mud resistance significantly improve their working performance.
Patent Information
- Application Number
- CN202410908912.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-22
AI Technical Summary
The high sand content in existing concrete and mortar leads to poor working performance and reduced strength, making it difficult to effectively solve this problem.
A sludge-resistant concrete water reducing agent, including 3-5 parts by weight of polycarboxylic acid water reducing agent, 1-3 parts by weight of quaternized silicone and 1-2 parts by weight of bentonite, through specific synthesis Methods: Quaternary silicas were prepared, combined with the stirring of polycarboxylic acid water reducing agent and bentonite to improve the compressive resistance and mud resistance of concrete.
It significantly improves the compactness, flexural strength and mud resistance of concrete, inhibits slump loss, improves the flowability and strength of concrete, and significantly improves the working performance of concrete.
Smart Images

Figure BDA0004932971450000091 
Figure BDA0004932971450000101 
Figure BDA0004932971450000102
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete, in particular to an anti-mud type concrete water reducing agent and a preparation method thereof. Background Art
[0002] In the production process of concrete and mortar, sand plays a vital role as the main raw material. The mud content of sand is an important indicator of sand performance and one of the most sensitive indicators affecting the performance of concrete and mortar. The mud content of sand directly affects the working performance of concrete and mortar. Too high mud content directly leads to poor workability and reduced strength of concrete and mortar. Therefore, how to avoid this phenomenon is the key to solving the problem. Summary of the invention
[0003] 1. Technical issues to be resolved
[0004] In view of the deficiencies of the prior art, the present invention provides an anti-mud type concrete water reducing agent and a preparation method thereof, which has good mud resistance and improves the compression resistance of concrete.
[0005] (II) Technical solution
[0006] To achieve the above object, the present invention provides the following technical solution: an anti-mud concrete water reducer, comprising the following weight components: 3-5 weight parts of polycarboxylate water reducer, 1-3 weight parts of quaternary ammonium siloxane, and 1-2 weight parts of bentonite.
[0007] Preferably, the preparation method of the quaternized siloxane is:
[0008] (1) Adding amino carbon nanotubes and benzophenone tetracarboxylic dianhydride to N,N-dimethylformamide solvent, stirring evenly, continuing to add pyridine catalyst, heating to 75-95° C., stirring and reacting for 15-30 hours, and after the reaction, concentrating under reduced pressure to remove the solvent, then washing the crude product with ether, and then dissolving the product in dichloromethane for recrystallization and purification to obtain intermediate 1;
[0009] (2) adding 3-dimethylaminopropanol and intermediate 1 to N,N-dimethylformamide solvent, stirring and mixing, and then adding p-toluenesulfonic acid catalyst thereto, reacting at 80-95° C. for 8-15 hours, and then distilling under reduced pressure, filtering and drying to obtain intermediate 2;
[0010] (3) adding allyloxy polyoxyethylene ether to N,N-dimethylformamide solvent, stirring to dissolve, adding platinum catalyst to it, heating to 70-95° C. to activate for 0.4-1.2 hours, then continuing to heat to 100-110° C., adding heptamethyl trisiloxane to it dropwise at a constant pressure, reacting at 100-115° C. for 4-8 hours after the addition, and then removing low-boiling substances by reduced pressure distillation to obtain polyether-modified trisiloxane;
[0011] (4) adding 2,2-bis(bromomethyl)-1,3-propylene glycol and polyether-modified trisiloxane to an acetone solvent, stirring evenly, and then continuing to add a 3-5 mol / L sodium hydroxide aqueous solution, reacting at 60-85° C. for 4-10 hours. After the reaction is completed, neutralizing, concentrating, filtering, washing and drying to obtain an intermediate 3;
[0012] (5) Add intermediate 3 and intermediate 2 to N,N-dimethylformamide solvent, stir and mix, continue to add dibutyltin dilaurate catalyst, react at 90-100° C. for 8-15 hours, and then distill under reduced pressure, filter and dry to obtain intermediate 4;
[0013] (6) Add intermediate 4 and chloroacetic acid to acetone solvent, stir and mix, then add 8-15% by mass sodium hydroxide solution, react at 80-120° C. for 2-4 hours, filter and dry after reaction to obtain quaternary ammonium siloxane.
[0014] Preferably, the mass ratio of the amino carbon nanotubes, benzophenonetetracarboxylic dianhydride and pyridine catalyst in (1) is 1.2-1.5:1:0.01-0.03.
[0015] Preferably, the mass ratio of 3-dimethylaminopropanol, intermediate 1, and p-toluenesulfonic acid catalyst in (2) is 1:1.1-1.2:0.02-0.03.
[0016] Preferably, the mass ratio of allyloxy polyoxyethylene ether, platinum catalyst and heptamethyl trisiloxane in (3) is 1:0.03-0.05:1.2-1.4.
[0017] Preferably, the mass ratio of 2,2-bis(bromomethyl)-1,3-propylene glycol to polyether-modified trisiloxane in (4) is 1.5-1.7:1.
[0018] Preferably, the mass ratio of intermediate 3, intermediate 2 and dibutyltin dilaurate catalyst in (5) is 1.6-1.8:1:0.01-0.04.
[0019] Preferably, the mass ratio of the intermediate 4 to chloroacetic acid in (6) is 1:1.5-1.9.
[0020] Preferably, the preparation method of the anti-mud concrete water reducer comprises the following steps: adding polycarboxylate water reducer, quaternized siloxane and bentonite into a stirrer, stirring at 60-90° C. for 10-15 minutes, and obtaining the anti-mud concrete water reducer after stirring.
[0021] (III) Beneficial technical effects
[0022] The invention adds polycarboxylate water-reducing agent, quaternized siloxane and bentonite into a stirrer, and stirs to obtain the anti-mud concrete water-reducing agent.
[0023] The carbon nanotubes contained in quaternary ammonium siloxane can interact physically or chemically with cement-based materials and enhance the mechanical properties of concrete through the nano effect. The silane contained in it can fill the voids in the concrete, thereby improving the density of the concrete, and also significantly improving the flexural strength of the concrete and improving the mud resistance of the concrete; quaternary ammonium salts improve the fluidity of concrete, inhibit slump loss, and improve the strength of concrete. DETAILED DESCRIPTION
[0024] Example 1
[0025] (1) Adding aminated carbon nanotubes and benzophenone tetracarboxylic acid dianhydride to N,N-dimethylformamide solvent, stirring evenly, and then adding pyridine catalyst, wherein the mass ratio of aminated carbon nanotubes, benzophenone tetracarboxylic acid dianhydride and pyridine catalyst is 1.2:1:0.01, heating to 75° C. and stirring for 15 hours, and after the reaction, concentrating under reduced pressure to remove the solvent, and then washing the crude product with ether, and then dissolving the product in dichloromethane for recrystallization and purification to obtain intermediate 1;
[0026] (2) adding 3-dimethylaminopropanol and intermediate 1 to N,N-dimethylformamide solvent, stirring and mixing, and then continuously adding p-toluenesulfonic acid catalyst thereto, wherein the mass ratio of 3-dimethylaminopropanol, intermediate 1, and p-toluenesulfonic acid catalyst is 1:1.1:0.02, reacting at 80° C. for 8 h, and then distilling under reduced pressure after the reaction, filtering and drying to obtain intermediate 2;
[0027] (3) adding allyloxy polyoxyethylene ether to N,N-dimethylformamide solvent, stirring to dissolve, continuing to add platinum catalyst thereto, heating to 70°C for activation for 0.4h, then continuing to heat to 100°C, adding heptamethyl trisiloxane thereto at a constant pressure, wherein the mass ratio of allyloxy polyoxyethylene ether, platinum catalyst and heptamethyl trisiloxane is 1:0.03:1.2, reacting at 100°C for 4h after the addition, and removing low boiling points by reduced pressure distillation to obtain polyether modified trisiloxane;
[0028] (4) adding 2,2-bis(bromomethyl)-1,3-propylene glycol and polyether-modified trisiloxane to an acetone solvent, wherein the mass ratio of 2,2-bis(bromomethyl)-1,3-propylene glycol to polyether-modified trisiloxane is 1.5:1, stirring evenly, and then continuing to add a 3 mol / L sodium hydroxide aqueous solution, reacting at 60° C. for 4 h. After the reaction is completed, neutralizing, concentrating, filtering, washing and drying to obtain an intermediate 3;
[0029] (5) adding intermediate 3 and intermediate 2 to N,N-dimethylformamide solvent, stirring and mixing, and continuously adding dibutyltin dilaurate catalyst thereto, wherein the mass ratio of intermediate 3, intermediate 2, and dibutyltin dilaurate catalyst is 1.6:1:0.01, reacting at 90° C. for 8 h, and then distilling under reduced pressure, filtering and drying to obtain intermediate 4;
[0030] (6) adding intermediate 4 and chloroacetic acid to an acetone solvent, wherein the mass ratio of intermediate 4 to chloroacetic acid is 1:1.5, stirring and mixing, and then adding 8% by mass sodium hydroxide solution thereto, reacting at 80° C. for 2 h, filtering and drying after completion, to obtain a quaternary ammonium siloxane;
[0031] (7) 3 parts by weight of polycarboxylate water-reducing agent, 1 part by weight of quaternized siloxane, and 1 part by weight of bentonite were added into a stirrer and stirred at 60° C. for 10 min to obtain an anti-mud concrete water-reducing agent.
[0032] Example 2
[0033] (1) Adding aminated carbon nanotubes and benzophenone tetracarboxylic acid dianhydride to N,N-dimethylformamide solvent, stirring evenly, and continuing to add pyridine catalyst, wherein the mass ratio of aminated carbon nanotubes, benzophenone tetracarboxylic acid dianhydride and pyridine catalyst is 1.5:1:0.03, heating to 95° C. and stirring for 30 hours, after the reaction, concentrating under reduced pressure to remove the solvent, then washing the crude product with ether, and then dissolving the product in dichloromethane for recrystallization and purification to obtain intermediate 1;
[0034] (2) adding 3-dimethylaminopropanol and intermediate 1 to N,N-dimethylformamide solvent, stirring and mixing, and then continuously adding p-toluenesulfonic acid catalyst thereto, wherein the mass ratio of 3-dimethylaminopropanol, intermediate 1, and p-toluenesulfonic acid catalyst is 1:1.2:0.03, reacting at 95° C. for 15 h, and then distilling under reduced pressure after the reaction, filtering and drying to obtain intermediate 2;
[0035] (3) adding allyloxy polyoxyethylene ether to N,N-dimethylformamide solvent, stirring to dissolve, continuing to add platinum catalyst thereto, heating to 95°C for activation for 1.2h, then continuing to heat to 110°C, adding heptamethyl trisiloxane thereto at a constant pressure, wherein the mass ratio of allyloxy polyoxyethylene ether, platinum catalyst, and heptamethyl trisiloxane is 1:0.05:1.4, reacting at 115°C for 8h after the addition is completed, and then removing low-boiling substances by reduced pressure distillation to obtain polyether-modified trisiloxane;
[0036] (4) adding 2,2-bis(bromomethyl)-1,3-propylene glycol and polyether-modified trisiloxane to an acetone solvent, wherein the mass ratio of 2,2-bis(bromomethyl)-1,3-propylene glycol to polyether-modified trisiloxane is 1.7:1, stirring evenly, and then continuing to add a 5 mol / L sodium hydroxide aqueous solution, reacting at 85° C. for 10 h. After the reaction is completed, neutralizing, concentrating, filtering, washing and drying to obtain an intermediate 3;
[0037] (5) adding intermediate 3 and intermediate 2 to N,N-dimethylformamide solvent, stirring and mixing, and continuously adding dibutyltin dilaurate catalyst thereto, wherein the mass ratio of intermediate 3, intermediate 2, and dibutyltin dilaurate catalyst is 1.8:1:0.04, reacting at 100° C. for 15 h, and then distilling under reduced pressure, filtering and drying to obtain intermediate 4;
[0038] (6) adding intermediate 4 and chloroacetic acid to an acetone solvent, wherein the mass ratio of intermediate 4 to chloroacetic acid is 1:1.9, stirring and mixing, and then adding a 15% sodium hydroxide solution to the mixture, reacting at 120° C. for 4 h, filtering and drying after the reaction to obtain a quaternary ammonium siloxane;
[0039] (7) 5 parts by weight of polycarboxylate water-reducing agent, 3 parts by weight of quaternized siloxane, and 2 parts by weight of bentonite were added into a stirrer and stirred at 90° C. for 15 minutes to obtain an anti-mud concrete water-reducing agent.
[0040] Example 3
[0041] (1) Adding aminated carbon nanotubes and benzophenone tetracarboxylic acid dianhydride to N,N-dimethylformamide solvent, stirring evenly, and continuing to add pyridine catalyst, wherein the mass ratio of aminated carbon nanotubes, benzophenone tetracarboxylic acid dianhydride and pyridine catalyst is 1.35:1:0.02, heating to 85° C. and stirring for 22.5 hours, and after the reaction, concentrating under reduced pressure to remove the solvent, and then washing the crude product with ether, and then dissolving the product in dichloromethane for recrystallization and purification to obtain intermediate 1;
[0042] (2) adding 3-dimethylaminopropanol and intermediate 1 to N,N-dimethylformamide solvent, stirring and mixing, and then continuously adding p-toluenesulfonic acid catalyst thereto, wherein the mass ratio of 3-dimethylaminopropanol, intermediate 1, and p-toluenesulfonic acid catalyst is 1:1.15:0.025, reacting at 87.5° C. for 11.5 hours, and then distilling under reduced pressure after the reaction, filtering and drying to obtain intermediate 2;
[0043] (3) adding allyloxy polyoxyethylene ether to N,N-dimethylformamide solvent, stirring to dissolve, continuing to add platinum catalyst thereto, heating to 82.5°C for activation for 0.8h, then continuing to heat to 105°C, adding heptamethyl trisiloxane thereto at a constant pressure, wherein the mass ratio of allyloxy polyoxyethylene ether, platinum catalyst, and heptamethyl trisiloxane is 1:0.04:1.3, reacting at 107.5°C for 6h after the addition is completed, and then removing low-boiling substances by reduced pressure distillation to obtain polyether-modified trisiloxane;
[0044] (4) adding 2,2-bis(bromomethyl)-1,3-propylene glycol and polyether-modified trisiloxane to an acetone solvent, wherein the mass ratio of 2,2-bis(bromomethyl)-1,3-propylene glycol to polyether-modified trisiloxane is 1.6:1, stirring evenly, and then continuing to add a 4 mol / L sodium hydroxide aqueous solution, reacting at 72.5° C. for 7 h. After the reaction is completed, neutralizing, concentrating, filtering, washing and drying to obtain an intermediate 3;
[0045] (5) adding intermediate 3 and intermediate 2 to N,N-dimethylformamide solvent, stirring and mixing, and continuously adding dibutyltin dilaurate catalyst thereto, wherein the mass ratio of intermediate 3, intermediate 2, and dibutyltin dilaurate catalyst is 1.7:1:0.0025, reacting at 95° C. for 11.5 h, and then distilling under reduced pressure, filtering and drying to obtain intermediate 4;
[0046] (6) adding intermediate 4 and chloroacetic acid to an acetone solvent, wherein the mass ratio of intermediate 4 to chloroacetic acid is 1:1.7, stirring and mixing, and then adding a sodium hydroxide solution with a mass fraction of 11.5%, reacting at 100° C. for 3 h, filtering and drying after completion, to obtain a quaternary ammonium siloxane;
[0047] (7) 4 parts by weight of polycarboxylate water-reducing agent, 2 parts by weight of quaternized siloxane, and 1.5 parts by weight of bentonite were added into a stirrer and stirred at 75° C. for 12.5 min to obtain an anti-mud concrete water-reducing agent.
[0048] Example 4
[0049] (1) Adding aminated carbon nanotubes and benzophenone tetracarboxylic acid dianhydride to N,N-dimethylformamide solvent, stirring evenly, and then adding pyridine catalyst, wherein the mass ratio of aminated carbon nanotubes, benzophenone tetracarboxylic acid dianhydride and pyridine catalyst is 1.2:1:0.01, heating to 75° C. and stirring for 15 hours, and after the reaction, concentrating under reduced pressure to remove the solvent, and then washing the crude product with ether, and then dissolving the product in dichloromethane for recrystallization and purification to obtain intermediate 1;
[0050] (2) adding 3-dimethylaminopropanol and intermediate 1 to N,N-dimethylformamide solvent, stirring and mixing, and then continuously adding p-toluenesulfonic acid catalyst thereto, wherein the mass ratio of 3-dimethylaminopropanol, intermediate 1, and p-toluenesulfonic acid catalyst is 1:1.1:0.02, reacting at 80° C. for 8 h, and then distilling under reduced pressure after the reaction, filtering and drying to obtain intermediate 2;
[0051] (3) adding allyloxy polyoxyethylene ether to N,N-dimethylformamide solvent, stirring to dissolve, continuing to add platinum catalyst thereto, heating to 95°C for activation for 1.2h, then continuing to heat to 110°C, adding heptamethyl trisiloxane thereto at a constant pressure, wherein the mass ratio of allyloxy polyoxyethylene ether, platinum catalyst, and heptamethyl trisiloxane is 1:0.05:1.4, reacting at 115°C for 8h after the addition is completed, and then removing low-boiling substances by reduced pressure distillation to obtain polyether-modified trisiloxane;
[0052] (4) adding 2,2-bis(bromomethyl)-1,3-propylene glycol and polyether-modified trisiloxane to an acetone solvent, wherein the mass ratio of 2,2-bis(bromomethyl)-1,3-propylene glycol to polyether-modified trisiloxane is 1.7:1, stirring evenly, and then continuing to add a 5 mol / L sodium hydroxide aqueous solution, reacting at 85° C. for 10 h. After the reaction is completed, neutralizing, concentrating, filtering, washing and drying to obtain an intermediate 3;
[0053] (5) adding intermediate 3 and intermediate 2 to N,N-dimethylformamide solvent, stirring and mixing, and continuously adding dibutyltin dilaurate catalyst thereto, wherein the mass ratio of intermediate 3, intermediate 2, and dibutyltin dilaurate catalyst is 1.7:1:0.0025, reacting at 95° C. for 11.5 h, and then distilling under reduced pressure, filtering and drying to obtain intermediate 4;
[0054] (6) adding intermediate 4 and chloroacetic acid to an acetone solvent, wherein the mass ratio of intermediate 4 to chloroacetic acid is 1:1.7, stirring and mixing, and then adding a sodium hydroxide solution with a mass fraction of 11.5%, reacting at 100° C. for 3 h, filtering and drying after completion, to obtain a quaternary ammonium siloxane;
[0055] (7) 4 parts by weight of polycarboxylate water-reducing agent, 2 parts by weight of quaternized siloxane, and 1.5 parts by weight of bentonite were added into a stirrer and stirred at 75° C. for 12.5 min to obtain an anti-mud concrete water-reducing agent.
[0056] Example 5
[0057] (1) Adding aminated carbon nanotubes and benzophenone tetracarboxylic acid dianhydride to N,N-dimethylformamide solvent, stirring evenly, and continuing to add pyridine catalyst, wherein the mass ratio of aminated carbon nanotubes, benzophenone tetracarboxylic acid dianhydride and pyridine catalyst is 1.5:1:0.03, heating to 95° C. and stirring for 30 hours, after the reaction, concentrating under reduced pressure to remove the solvent, then washing the crude product with ether, and then dissolving the product in dichloromethane for recrystallization and purification to obtain intermediate 1;
[0058] (2) adding 3-dimethylaminopropanol and intermediate 1 to N,N-dimethylformamide solvent, stirring and mixing, and then continuously adding p-toluenesulfonic acid catalyst thereto, wherein the mass ratio of 3-dimethylaminopropanol, intermediate 1, and p-toluenesulfonic acid catalyst is 1:1.2:0.03, reacting at 95° C. for 15 h, and then distilling under reduced pressure after the reaction, filtering and drying to obtain intermediate 2;
[0059] (3) adding allyloxy polyoxyethylene ether to N,N-dimethylformamide solvent, stirring to dissolve, continuing to add platinum catalyst thereto, heating to 82.5°C for activation for 0.8h, then continuing to heat to 105°C, adding heptamethyl trisiloxane thereto at a constant pressure, wherein the mass ratio of allyloxy polyoxyethylene ether, platinum catalyst, and heptamethyl trisiloxane is 1:0.04:1.3, reacting at 107.5°C for 6h after the addition is completed, and then removing low-boiling substances by reduced pressure distillation to obtain polyether-modified trisiloxane;
[0060] (4) adding 2,2-bis(bromomethyl)-1,3-propylene glycol and polyether-modified trisiloxane to an acetone solvent, wherein the mass ratio of 2,2-bis(bromomethyl)-1,3-propylene glycol to polyether-modified trisiloxane is 1.6:1, stirring evenly, and then continuing to add a 4 mol / L sodium hydroxide aqueous solution, reacting at 72.5° C. for 7 h. After the reaction is completed, neutralizing, concentrating, filtering, washing and drying to obtain an intermediate 3;
[0061] (5) adding intermediate 3 and intermediate 2 to N,N-dimethylformamide solvent, stirring and mixing, and continuously adding dibutyltin dilaurate catalyst thereto, wherein the mass ratio of intermediate 3, intermediate 2, and dibutyltin dilaurate catalyst is 1.6:1:0.01, reacting at 90° C. for 8 h, and then distilling under reduced pressure, filtering and drying to obtain intermediate 4;
[0062] (6) adding intermediate 4 and chloroacetic acid to an acetone solvent, wherein the mass ratio of intermediate 4 to chloroacetic acid is 1:1.5, stirring and mixing, and then adding 8% by mass sodium hydroxide solution thereto, reacting at 80° C. for 2 h, filtering and drying after completion, to obtain a quaternary ammonium siloxane;
[0063] (7) 3 parts by weight of polycarboxylate water-reducing agent, 1 part by weight of quaternized siloxane, and 1 part by weight of bentonite were added into a stirrer and stirred at 60° C. for 10 min to obtain an anti-mud concrete water-reducing agent.
[0064] Comparative Example 1
[0065] (1) 3 parts by weight of polycarboxylate water reducer and 1 part by weight of bentonite were added into a stirrer and stirred at 60° C. for 10 min to obtain an anti-mud concrete water reducer.
[0066] Performance Testing
[0067] At 20-40℃, pour medium sand and gravel into a mixer and stir for 2-3min, then add fly ash and cement and continue stirring for 5-10min, pour the anti-mud concrete water reducer into the water, stir evenly, then slowly add water to the stirred mixture, continue stirring for 4-5min, after completion, cast into a mold, cure at room temperature for 20-22h, remove the mold after forming, and then cure in a standard curing room for 30-32 days to obtain a concrete specimen.
[0068] The mortar fluidity test is carried out according to GB / T8077-2012 "Test method for homogeneity of concrete admixtures".
[0069] Table 1: Flowability test.
[0070]
[0071]
[0072] It can be seen from Table 1 that Examples 1-5 of the present invention have better fluidity than Comparative Example 1, indicating that the anti-mud effect is better.
[0073] According to the flexural strength test in GB / T50081-2002 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete", the 7d flexural strength (MPa) and 28d flexural strength (MPa) of the high-strength flexural concrete samples prepared in each embodiment and comparative example were tested.
[0074] Table 2: Flexural strength test.
[0075] project 7d flexural strength (MPa) 28d flexural strength (MPa) Example 1 5.6 5.8 Example 2 6.3 6.5 Example 3 5.8 6.2 Example 4 5.9 6.2 Example 5 6.2 6.3 Comparative Example 1 4.1 4.0
[0076] It can be seen from Table 2 that Examples 1-5 of the present invention have better flexural strength than Comparative Example 1.
[0077] Test product collapse according to GB / 8076-2008.
[0078] Table 3: Slump test.
[0079]
[0080]
[0081] As can be seen from Table 3, compared with Comparative Example 1, the slump changes of Examples 1-5 of the present invention are smaller, and the change of the comparative example is the largest.
[0082] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A mud-resistant concrete water reducer, characterized in that: The invention comprises the following components by weight: 3-5 parts by weight of polycarboxylate water-reducing agent, 1-3 parts by weight of quaternary ammonium siloxane and 1-2 parts by weight of bentonite.
2. The anti-mud concrete water reducing agent according to claim 1, characterized in that: The preparation method of the quaternized siloxane is: (1) Adding amino carbon nanotubes and benzophenone tetracarboxylic dianhydride to N,N-dimethylformamide solvent, stirring evenly, continuing to add pyridine catalyst, heating to 75-95° C., stirring and reacting for 15-30 hours, and after the reaction, concentrating under reduced pressure to remove the solvent, then washing the crude product with ether, and then dissolving the product in dichloromethane for recrystallization and purification to obtain intermediate 1; (2) adding 3-dimethylaminopropanol and intermediate 1 to N,N-dimethylformamide solvent, stirring and mixing, and then adding p-toluenesulfonic acid catalyst thereto, reacting at 80-95° C. for 8-15 hours, and then distilling under reduced pressure, filtering and drying to obtain intermediate 2; (3) adding allyloxy polyoxyethylene ether to N,N-dimethylformamide solvent, stirring to dissolve, adding platinum catalyst to it, heating to 70-95° C. to activate for 0.4-1.2 hours, then continuing to heat to 100-110° C., adding heptamethyl trisiloxane to it dropwise at a constant pressure, reacting at 100-115° C. for 4-8 hours after the addition, and then removing low-boiling substances by reduced pressure distillation to obtain polyether-modified trisiloxane; (4) adding 2,2-bis(bromomethyl)-1,3-propylene glycol and polyether-modified trisiloxane to an acetone solvent, stirring evenly, and then continuing to add a 3-5 mol / L sodium hydroxide aqueous solution, reacting at 60-85° C. for 4-10 hours. After the reaction is completed, neutralizing, concentrating, filtering, washing and drying to obtain an intermediate 3; (5) Add intermediate 3 and intermediate 2 to N,N-dimethylformamide solvent, stir and mix, continue to add dibutyltin dilaurate catalyst, react at 90-100° C. for 8-15 hours, and then distill under reduced pressure, filter and dry to obtain intermediate 4; (6) Add intermediate 4 and chloroacetic acid to acetone solvent, stir and mix, then add 8-15% by mass sodium hydroxide solution, react at 80-120° C. for 2-4 hours, filter and dry after reaction to obtain quaternary ammonium siloxane.
3. The anti-mud concrete water reducing agent according to claim 2, characterized in that: The mass ratio of the amino carbon nanotubes, benzophenonetetracarboxylic acid dianhydride and pyridine catalyst in (1) is 1.2-1.5:1:0.01-0.
03.
4. The anti-mud concrete water reducing agent according to claim 2, characterized in that: The mass ratio of 3-dimethylaminopropanol, intermediate 1 and p-toluenesulfonic acid catalyst in (2) is 1:1.1-1.2:0.02-0.
03.
5. The anti-mud concrete water reducing agent according to claim 2, characterized in that: The mass ratio of allyloxy polyoxyethylene ether, platinum catalyst and heptamethyl trisiloxane in (3) is 1:0.03-0.05:1.2-1.
4.
6. The anti-mud concrete water reducing agent according to claim 2, characterized in that: The mass ratio of 2,2-bis(bromomethyl)-1,3-propylene glycol to polyether-modified trisiloxane in (4) is 1.5-1.7:
1.
7. The anti-mud concrete water reducing agent according to claim 2, characterized in that: The mass ratio of intermediate 3, intermediate 2 and dibutyltin dilaurate catalyst in (5) is 1.6-1.8:1:0.01-0.
04.
8. The anti-mud concrete water reducing agent according to claim 2, characterized in that: The mass ratio of the intermediate 4 to chloroacetic acid in (6) is 1:1.5-1.
9.
9. A method for preparing the anti-mud concrete water reducing agent according to any one of claims 1 to 8, characterized in that: The preparation method of the anti-mud concrete water reducer comprises the following steps: adding polycarboxylic acid water reducer, quaternary ammonium siloxane and bentonite into a stirrer, stirring at 60-90° C. for 10-15 minutes, and obtaining the anti-mud concrete water reducer after stirring.