Anti-freezing anti-cracking polylactic acid fiber concrete and preparation method thereof
Through the synergistic effect of nano-silica, silurea copolymer and phosphate, an antifreeze stabilizer is formed, which solves the problem of degradation of freeze-thaw cycle of polylactic fiber concrete in cold areas, and significantly improves the freeze-resistant and mechanical properties. Extend the service life of concrete.
Patent Information
- Application Number
- CN202411129342.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing polylactic fiber concrete degrades rapidly under the freeze-thaw cycle in cold areas, resulting in a decrease in mechanical properties, poor anti-freeze-resistant and cracking effects, and unstable local performance.
Nanosilicon dioxide and silicurea copolymer are used to form a mesh structure, combined with phosphate, and antifreeze stabilizer is prepared. By capturing and fixing moisture, ice crystal formation is reduced, concrete antifreeze ability is enhanced, and compaction is improved by in-depth filling of micropores. and structural strength.
It significantly improves the frost resistance, mechanical properties and permeability of concrete, extends the service life, slows down the degradation process of polylactic fibers, and enhances the integrity and durability of the structure.
Smart Images

Figure BDA0004997371230000091 
Figure BDA0004997371230000092
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of concrete, and specifically relates to a frost-resistant and crack-resistant polylactic acid fiber concrete and a preparation method thereof. Background Art
[0002] As one of the most commonly used materials in building structures, the stability of concrete performance is of vital importance for the long-term use and maintenance of buildings. However, in cold areas, concrete will be subjected to a large number of freeze-thaw cycles, resulting in cracking, peeling and other damage to the concrete, which will seriously affect the service life of the building structure and the safety of the occupants. Although traditional concrete has high strength and durability, its performance is often greatly reduced when facing extreme cold climate conditions. Especially in northern regions or high-altitude cold areas, the low temperature in winter and the freeze-thaw cycle when the ice and snow melt pose a severe challenge to the stability of concrete structures. Polylactic acid fiber, referred to as PLA fiber, is a fiber material made from crops such as corn through a series of chemical and physical processing. It not only has reliable biosafety and biodegradability, but also exhibits good mechanical properties. Adding polylactic acid fiber to concrete can effectively improve the internal structure of concrete and enhance its toughness and crack resistance. Especially in the face of freeze-thaw cycles, polylactic acid fiber can effectively inhibit the generation and development of microcracks inside concrete, thereby improving the freeze-thaw resistance of concrete. For example, the Chinese patent publication number CN113788655B is a kind of antifreeze and anti-cracking concrete and its preparation method, the raw materials include cementitious materials, aggregates, fly ash, polycarboxylic acid water reducer, antifreeze agent, mixing water, sepiolite-polylactic acid composite fiber and modified mesoporous silica, wherein the sepiolite-polylactic acid composite fiber is composed of sepiolite fiber and polylactic acid fiber, and a large number of small bubbles are evenly distributed in the structure, which can effectively improve the antifreeze and anti-cracking properties.
[0003] In the prior art, the degradation of polylactic acid fiber is mainly through the action of microbial enzymes, which causes the polylactic acid molecular chain to break into small molecule lactic acid, which is further metabolized into carbon dioxide and water. This process is slow in the natural environment, but under specific conditions inside the concrete, the degradation rate will be accelerated. Concrete is usually alkaline. Under alkaline conditions, the hydrolysis reaction of the ester group will be accelerated, causing the polylactic acid fiber to decompose into small molecule lactic acid faster. At the same time, the bubbles in the concrete provide a good living space for microorganisms, allowing microorganisms to reproduce rapidly inside the concrete, increasing the degradation rate of polylactic acid. As the polylactic acid fiber degrades, the concrete part originally reinforced by it will lose support, resulting in microscopic or macroscopic cracks inside the concrete, which in turn affects the integrity of the structure. The degradation of polylactic acid fiber will cause the mechanical properties of concrete (such as compressive strength, tensile strength, etc.) to gradually decrease. In addition, the local performance of some polylactic acid fiber concrete is unstable, and the anti-freeze and anti-cracking effects are poor. Summary of the invention
[0004] The object of the present invention is to provide a frost-resistant and crack-resistant polylactic acid fiber concrete and a preparation method thereof in view of the deficiencies in the prior art.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A frost-resistant and crack-resistant polylactic acid fiber concrete comprises the following raw materials by weight: 5-10 parts of polylactic acid fibers, 450-500 parts of cement, 200-400 parts of fine sand and gravel, 30-50 parts of silica fume, 1-3 parts of polycarboxylic acid high-performance water reducing agent, 6-24 parts of antifreeze stabilizer, 1-3 parts of polyvinyl alcohol and 100-200 parts of water.
[0007] Preferably, the following raw materials are included by weight: 5-8 parts of polylactic acid fiber, 450-475 parts of cement, 250-400 parts of fine sand and gravel, 30-45 parts of silica fume, 1-2 parts of polycarboxylic acid high-performance water reducing agent, 6-18 parts of antifreeze stabilizer, 1-2 parts of polyvinyl alcohol and 120-200 parts of water.
[0008] Preferably, the following raw materials are included by weight: 5-7 parts of polylactic acid fiber, 450-460 parts of cement, 250-300 parts of fine sand and gravel, 36-40 parts of silica fume, 1 part of polycarboxylic acid high-performance water reducer, 10-16 parts of antifreeze stabilizer, 2 parts of polyvinyl alcohol and 140-160 parts of water.
[0009] Furthermore, the antifreeze stabilizer is prepared by the following steps:
[0010] S1. Mix trimethoxysilane and urea propionic acid and put them into a reaction container. Under nitrogen protection, heat the reaction container to 80-90° C., stir continuously at a stirring speed of 400-500 rpm for 2-4 hours, cool to room temperature, filter, and wash to obtain a silylurea copolymer.
[0011] S2, dispersing nano-silicon dioxide in methanol, stirring continuously at 300-400 rpm at 60-70° C. for 1-2 h, and ultrasonically treating for 20-30 min to obtain a nano-silicon dioxide dispersion;
[0012] S3. Mix the nano-silica dispersion and the silane urea copolymer, add phosphate, heat to 120-140°C under nitrogen gas protection, continue stirring at a speed of 600-800 rpm, react for 4-6 hours, and after the reaction is completed, cool to room temperature, filter, wash, and dry to obtain an antifreeze stabilizer.
[0013] The usage ratio of trimethoxysilane and urea propionic acid in step S1 is (12-18) mL: (5-7) g.
[0014] In the step S2, the dosage ratio of nano-silicon dioxide to methanol is (8-18) g: (50-60) mL, the frequency of ultrasonic treatment is 45-55 kHz, and the power is 200-250 W.
[0015] In the step S3, the dosage ratio of the nano-silica dispersion, the silicourea copolymer and the phosphate is (14-20) mL: (8-12) g: (2-7) g, and the phosphate includes one or more of sodium phosphate, calcium phosphate, iron phosphate, aluminum phosphate and zinc phosphate.
[0016] According to another aspect of the present invention, a method for preparing the above-mentioned frost-resistant and crack-resistant polylactic acid fiber concrete is provided, comprising the following steps:
[0017] Weigh fine sand, silica fume and cement by weight and put them into a concrete mixer, mix at 100-150rpm for 10-15min, cut the polylactic acid fiber into a length of 1-3cm, add it to the mixture, add polycarboxylic acid high-performance water reducer, antifreeze stabilizer and polyvinyl alcohol at the same time, stir at 300-400rpm for 5-10min, gradually add water during continuous stirring, each time adding no more than 1 / 3 of the total amount, and the interval between adding water is 1-2min. After adding water, stir at 150-200rpm until the concrete has no obvious particles and lumps.
[0018] Beneficial effects of the present invention:
[0019] 1. In the technical solution of the present invention, the mesh structure formed by nano-silica and silicourea copolymer effectively captures and fixes water, greatly inhibiting the formation and expansion of ice crystals, especially during the freeze-thaw cycle, significantly reducing the damage of ice crystals to the concrete structure, thereby greatly improving the frost resistance of concrete. In addition, the addition of phosphates reduces the freezing point of the solution by combining with metal ions in concrete, further enhancing the material's frost resistance.
[0020] 2. The nano-silicon dioxide particles used in the present invention can deeply fill the micropores and cracks inside the concrete, greatly improving the compactness and integrity of the concrete, thereby significantly enhancing its mechanical properties. The mesh structure formed by the siloxane urea copolymer inside the concrete not only enhances the cohesion of the concrete, but also closely connects with other components in the concrete through chemical bonding, thereby improving the structural strength and crack resistance of the concrete. While enhancing the interfacial bonding force, it can also effectively prevent moisture and microorganisms from eroding the polylactic acid fiber, thereby slowing down its degradation process.
[0021] 3. The concrete of the present invention has excellent anti-permeability and can effectively prevent the erosion of moisture and harmful gases, thereby significantly extending the service life of concrete. The small size effect of nano-silicon dioxide enables it to deeply fill the tiny pores in the concrete, enhance the compactness of the concrete, and further prevent the invasion of external moisture and microorganisms. Phosphates can combine with metal ions in concrete to form stable compounds, reduce the concentration of free ions, not only improve the durability of concrete, but also indirectly protect polylactic acid fibers from the effects of alkaline environments and microorganisms. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0023] Example 1
[0024] The antifreeze stabilizer is prepared by the following steps:
[0025] S1. Mix 120 mL of trimethoxysilane and 50 g of urea propionic acid and put them into a reaction container. Under nitrogen protection, heat the reaction container to 80° C. and continue stirring at 400 rpm for 2 h. Cool to room temperature, filter, and wash to obtain a silylurea copolymer.
[0026] S2, dispersing 80 g of nano-silicon dioxide in 500 mL of methanol, stirring continuously at 300 rpm for 1 h at 60 ° C, and ultrasonically treating for 20 min at a frequency of 45 kHz and a power of 200 W to obtain a nano-silicon dioxide dispersion;
[0027] S3. Mix 140 mL of nano-silica dispersion with 80 g of silicourea copolymer, add 20 g of aluminum phosphate, heat to 120°C under nitrogen protection, stir continuously at 600 rpm, react for 4 hours, and after the reaction is completed, cool to room temperature, filter, wash, and dry to obtain an antifreeze stabilizer.
[0028] Example 2
[0029] The antifreeze stabilizer is prepared by the following steps:
[0030] S1. Mix 150 mL of trimethoxysilane and 60 g of urea propionic acid and put them into a reaction container. Under nitrogen protection, heat the reaction container to 85° C. and continue stirring at a stirring speed of 450 rpm for 3 hours. Cool to room temperature, filter, and wash to obtain a silylurea copolymer.
[0031] S2, disperse 130g of nano-silicon dioxide in 550mL of methanol, stir continuously at 350rpm for 1.5h at 65°C, and ultrasonically treat for 25min at a frequency of 50kHz and a power of 225W to obtain a nano-silicon dioxide dispersion;
[0032] S3. Mix 170 mL of nano-silica dispersion with 100 g of silicourea copolymer, add 45 g of aluminum phosphate, heat to 130°C under nitrogen protection, stir continuously at 700 rpm, react for 5 hours, and after the reaction is completed, cool to room temperature, filter, wash, and dry to obtain an antifreeze stabilizer.
[0033] Example 3
[0034] The antifreeze stabilizer is prepared by the following steps:
[0035] S1. Mix 180 mL of trimethoxysilane and 70 g of urea propionic acid and put them into a reaction container. Under nitrogen protection, heat the reaction container to 90° C. and continue stirring at 500 rpm for 4 hours. Cool to room temperature, filter, and wash to obtain a silylurea copolymer.
[0036] S2, dispersing 180 g of nano-silicon dioxide in 600 mL of methanol, stirring continuously at 400 rpm for 2 h at 70 ° C, and ultrasonically treating for 30 min at a frequency of 55 kHz and a power of 250 W to obtain a nano-silicon dioxide dispersion;
[0037] S3. Mix 200 mL of nano-silica dispersion with 120 g of silicourea copolymer, add 70 g of aluminum phosphate, heat to 140°C under nitrogen protection, stir continuously at 800 rpm, react for 6 hours, and after the reaction is completed, cool to room temperature, filter, wash, and dry to obtain an antifreeze stabilizer.
[0038] Example 4
[0039] The preparation method of antifreeze and anti-cracking polylactic acid fiber concrete comprises the following steps:
[0040] 200 parts of fine sand and gravel, 30 parts of silica fume and 450 parts of cement were weighed by weight and put into a concrete mixer, mixed at 100 rpm for 10 min, 5 parts of polylactic acid fibers were cut to a length of 1 cm and added to the mixture, and 1 part of polycarboxylic acid high-performance water reducer, 6 parts of antifreeze stabilizer prepared in Example 1 and 1 part of polyvinyl alcohol were added at the same time, and stirred at 300 rpm for 5 min. During the continuous stirring process, 100 parts of water were gradually added, each time adding 1 / 3 of the total amount of water, and the interval between adding water was 1 min. After adding water, the concrete was stirred at 150 rpm until there were no obvious particles and lumps.
[0041] Example 5
[0042] The preparation method of antifreeze and anti-cracking polylactic acid fiber concrete comprises the following steps:
[0043] 300 parts of fine sand and gravel, 40 parts of silica fume and 475 parts of cement were weighed by weight and put into a concrete mixer, mixed at 125 rpm for 12.5 min, 7.5 parts of polylactic acid fibers were cut to a length of 2 cm and added to the mixture, and 2 parts of polycarboxylic acid high-performance water reducer, 15 parts of antifreeze stabilizer prepared in Example 2 and 2 parts of polyvinyl alcohol were added at the same time, and stirred at 350 rpm for 7.5 min. During the continuous stirring process, 150 parts of water were gradually added, each time adding 1 / 3 of the total amount of water, and the interval between adding water was 1.5 min. After adding water, the concrete was stirred at 175 rpm until there were no obvious particles and lumps.
[0044] Example 6
[0045] The preparation method of antifreeze and anti-cracking polylactic acid fiber concrete comprises the following steps:
[0046] 400 parts of fine sand and gravel, 50 parts of silica fume and 500 parts of cement were weighed by weight and put into a concrete mixer, mixed at 150 rpm for 15 min, 10 parts of polylactic acid fibers were cut to a length of 3 cm and added to the mixture, and 3 parts of polycarboxylic acid high-performance water reducer, 24 parts of the antifreeze stabilizer prepared in Example 3 and 3 parts of polyvinyl alcohol were added at the same time, and stirred at 400 rpm for 10 min. During the continuous stirring process, 200 parts of water were gradually added, each time adding 1 / 3 of the total amount of water, and the interval between adding water was 2 min. After adding water, the concrete was stirred at 200 rpm until there were no obvious particles and lumps.
[0047] Comparative Example 1
[0048] The difference between this comparative example and Example 1 is that trimethoxysilane is not added, and the remaining steps are the same as those of Example 1.
[0049] Comparative Example 2
[0050] The difference between this comparative example and Example 2 is that urea propionic acid is not added, and the remaining steps are the same as those in Example 2.
[0051] Comparative Example 3
[0052] The difference between this comparative example and Example 4 is that the composite prepared in Comparative Example 1 is added, and the remaining steps are the same as those in Example 4.
[0053] Comparative Example 4
[0054] The difference between this comparative example and Example 5 is that the composite prepared in Comparative Example 2 is added, and the remaining steps are the same as those in Example 5.
[0055] Comparative Example 5
[0056] The difference between this comparative example and Example 6 is that no antifreeze stabilizer is added, and the remaining steps are the same as those of Example 6.
[0057] The concrete samples prepared in Examples 4-6 and Comparative Examples 3-5 were tested with reference to GB / T 41054-2021 "Technical Conditions for High Performance Concrete", and the results are shown in Table 1:
[0058] Table 1. Performance test results of Examples 4-6 and Comparative Examples 3-5
[0059]
[0060] The concrete samples obtained in Examples 4-6 and Comparative Examples 3-5 were tested for compressive strength and flexural strength, and the cracking performance was tested using a four-point bending test. The results are shown in Table 2:
[0061] Table 2. Mechanical properties test results of Examples 4-6 and Comparative Examples 3-5
[0062]
[0063] The concrete samples prepared in Examples 4-6 and Comparative Examples 3-5 were placed in a freezing device and subjected to 100 freeze-thaw cycles, each cycle comprising freezing at -20°C for 8 hours and then thawing at 20°C for 8 hours. The surface damage of the concrete samples prepared in Examples 4-6 was no damage, the surface damage of the concrete samples prepared in Comparative Examples 3-4 exceeded 50%, and the surface was severely damaged, while the surface of the concrete sample prepared in Comparative Example 5 was completely damaged.
[0064] As can be seen from Tables 1 and 2, the concrete samples of Examples 4-6 all showed lower values in terms of chloride ion migration coefficient, electric flux and carbonation depth, indicating that these samples had better anti-permeability and durability. In contrast, the samples of Comparative Examples 3-5 performed poorly in these indicators, especially Comparative Example 5, which had the highest indicators, showing very poor anti-permeability and durability.
[0065] The samples of Examples 4-6 achieved relatively high values in the compressive strength, flexural strength and maximum bearing capacity tests, indicating that these concrete samples have relatively high structural strength and toughness. The samples of Comparative Examples 3-5 performed significantly worse in these mechanical property tests, especially Comparative Example 5, whose various mechanical property indicators were the lowest.
[0066] The samples of Examples 4-6 had no surface damage after 100 freeze-thaw cycles, showing excellent frost resistance. The samples of Comparative Examples 3-4 had serious surface damage after freeze-thaw cycles, and the sample of Comparative Example 5 was even completely damaged, indicating poor frost resistance.
[0067] The antifreeze stabilizer in the embodiment significantly improves the anti-permeability, durability and anti-freeze of concrete by enhancing the bonding force inside the concrete and filling micropores. This is due to the synergistic effect of the silane urea copolymer with nano silicon dioxide and aluminum phosphate. The lack of trimethoxysilane (Comparative Example 1) or urea propionic acid (Comparative Example 2) will cause the effect of the antifreeze stabilizer to drop significantly. Trimethoxysilane may be involved in the formation of the silane urea copolymer, enhancing the bonding force inside the concrete; while urea propionic acid may provide additional carboxyl groups, enhancing the interaction with the concrete matrix. Polylactic acid fiber plays a role in bridging microcracks and preventing crack expansion in concrete, thereby improving the flexural strength and cracking performance of concrete. No antifreeze stabilizer was added in Comparative Example 5, resulting in the worst performance indicators. It shows that the antifreeze stabilizer plays a key role in improving the performance of concrete. Concrete without antifreeze stabilizer is very vulnerable to damage during freeze-thaw cycles because it lacks sufficient bonding force and anti-permeability inside.
[0068] In summary, the concrete prepared in Examples 4-6 has good anti-permeability, durability, frost resistance and mechanical properties.
[0069] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0070] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A frost-resistant and crack-resistant polylactic acid fiber concrete, characterized in that: The raw materials include the following by weight: 5-10 parts of polylactic acid fiber, 450-500 parts of cement, 200-400 parts of fine sand and gravel, 30-50 parts of silica fume, 1-3 parts of polycarboxylic acid high-performance water reducing agent, 6-24 parts of antifreeze stabilizer, 1-3 parts of polyvinyl alcohol and 100-200 parts of water.
2. The antifreeze and anti-cracking polylactic acid fiber concrete according to claim 1, characterized in that: The raw materials include the following by weight: 5-8 parts of polylactic acid fiber, 450-475 parts of cement, 250-400 parts of fine sand and gravel, 30-45 parts of silica fume, 1-2 parts of polycarboxylic acid high-performance water reducing agent, 6-18 parts of antifreeze stabilizer, 1-2 parts of polyvinyl alcohol and 120-200 parts of water.
3. The antifreeze and anti-cracking polylactic acid fiber concrete according to claim 1, characterized in that: The raw materials include the following by weight: 5-7 parts of polylactic acid fiber, 450-460 parts of cement, 250-300 parts of fine sand and gravel, 36-40 parts of silica fume, 1 part of polycarboxylic acid high-performance water reducing agent, 10-16 parts of antifreeze stabilizer, 2 parts of polyvinyl alcohol and 140-160 parts of water.
4. The antifreeze and anti-cracking polylactic acid fiber concrete according to claim 1, characterized in that: The antifreeze stabilizer is prepared by the following steps: S1. Mix trimethoxysilane and urea propionic acid and put them into a reaction container. Under nitrogen protection, heat the reaction container to 80-90° C., stir continuously at a stirring speed of 400-500 rpm for 2-4 hours, cool to room temperature, filter, and wash to obtain a silylurea copolymer. S2, dispersing nano-silicon dioxide in methanol, stirring continuously at 300-400 rpm at 60-70° C. for 1-2 h, and ultrasonically treating for 20-30 min to obtain a nano-silicon dioxide dispersion; S3. Mix the nano-silica dispersion and the silane urea copolymer, add phosphate, heat to 120-140°C under nitrogen gas protection, continue stirring at a speed of 600-800 rpm, react for 4-6 hours, and after the reaction is completed, cool to room temperature, filter, wash, and dry to obtain an antifreeze stabilizer.
5. The antifreeze and anti-cracking polylactic acid fiber concrete according to claim 4, characterized in that: The usage ratio of trimethoxysilane and urea propionic acid in step S1 is (12-18) mL: (5-7) g.
6. The antifreeze and anti-cracking polylactic acid fiber concrete according to claim 4, characterized in that: In step S2, the dosage ratio of nano-silicon dioxide and methanol is (8-18) g: (50-60) mL, the frequency of ultrasonic treatment is 45-55 kHz, and the power is 200-250 W.
7. The antifreeze and anti-cracking polylactic acid fiber concrete according to claim 4, characterized in that: In step S3, the usage ratio of the nano-silica dispersion, the silicon urea copolymer and the phosphate is (14-20) mL: (8-12) g: (2-7) g, and the phosphate includes one or more of sodium phosphate, calcium phosphate, iron phosphate, aluminum phosphate and zinc phosphate.
8. The method for preparing a frost-resistant and crack-resistant polylactic acid fiber concrete according to any one of claims 1 to 7, characterized in that: The following steps are involved: Weigh fine sand, silica fume and cement by weight and put them into a concrete mixer, mix at 100-150rpm for 10-15min, cut the polylactic acid fiber into a length of 1-3cm, add it to the mixture, add polycarboxylic acid high-performance water reducer, antifreeze stabilizer and polyvinyl alcohol at the same time, stir at 300-400rpm for 5-10min, gradually add water during continuous stirring, each time adding no more than 1 / 3 of the total amount, and the interval between adding water is 1-2min. After adding water, stir at 150-200rpm until the concrete has no obvious particles and lumps.
Citation Information
Cited By
A foam concrete reinforced with hooked fiber made from PLA+
WO2026127840A1
Wavy PLA+ fiber reinforced and expanded glass aggregate added foam concrete
WO2026127841A1