High-crack-resistance wear-resistant self-leveling mortar

By using materials such as crack-resistant high-strength cement clinker, heavy calcium powder, modified steel slag powder, etc., the surface powdering and cracking of cement-based self-leveling mortar is solved, the crack resistance and wear resistance of the mortar is improved, and high efficiency is achieved construction performance and building quality improvement.

CN118993676AActive Publication Date: 2024-11-22JIAHUA SPECIAL CEMENT
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411075219.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The existing cement-based self-leveling mortar has quality problems such as surface pulverization and cracking during construction, and has poor wear resistance, which affects the appearance and use effect of the building.

Method used

Using crack-resistant high-strength cement clinker, heavy calcium powder, modified steel slag powder, gypsum, redispersible latex powder, powdered polycarboxylic acid water reducer and cellulose ether, high-strength materials are prepared through specific calcining and grinding processes. Cracking and wear resistance self-leveling mortar improves crack resistance and wear resistance of mortar.

Benefits of technology

It significantly improves the crack resistance and wear resistance of self-leveling mortar, reduces the shrinkage and dry shrinkage of the mortar, enhances the compactness and cohesion of the mortar, and meets the special requirements of low shrinkage and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004982017240000081
    Figure BDA0004982017240000081
  • Figure BDA0004982017240000091
    Figure BDA0004982017240000091
Patent Text Reader

Abstract

The invention discloses high-crack-resistance wear-resistant self-leveling mortar, which is prepared from the following raw materials in percentage by weight: 15 to 25 weight percent of crack-resistance Portland cement clinker, 5 to 10 weight percent of auxiliary cementing material, 3 to 7 weight percent of gypsum, 5 to 10 weight percent of heavy calcium powder, 3 to 7 weight percent of modified steel slag powder, 30 to 35 weight percent of 40 to 70-mesh quartz sand and 20 to 25 weight percent of 70 to 120-mesh quartz sand, the auxiliary materials account for the total mass percentage of the raw materials: 0.1-0.8 wt% of redispersible latex powder, 0.2-0.4 wt% of a powdery polycarboxylic acid water reducing agent, 0.01-0.02 wt% of cellulose ether and 0.1 wt% of a defoaming agent. The crack resistance and wear resistance of the self-leveling mortar are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a highly crack-resistant and wear-resistant self-leveling mortar. Background Art

[0002] Generally, the ground construction method is to mix ordinary Portland cement with sand, and then spread, scrape and plaster it manually. Before the mortar is finally set, three times of calendering and other processes must be completed. This multi-layer construction method has low production efficiency and large material waste. The ground after construction often has quality problems such as sanding, peeling, hollowing, and cracking, which seriously affects the appearance and use effect of the building. It has become a common quality problem of ordinary cement mortar floors and has not been effectively cured. In response to the above problems, cement-based self-leveling mortar has developed. It is a kind of cement-based self-leveling mortar that uses cement as the main cementing material, adds aggregates such as quartz sand and powdered fillers, and uses various chemical additives for modification. It is mixed evenly through the production process to become a powdered product. At present, there are mainly two types of cementing systems used in domestically produced cement-based self-leveling mortars: one is based on ordinary Portland cement, supplemented by aluminate cement and gypsum; the other is based on sulphoaluminate cement, supplemented by Portland cement and gypsum, but self-leveling mortar still has problems of surface powdering and cracking.

[0003] To solve the above problems, the invention patent is named "A self-leveling mortar and its preparation method and application", with application number CN202410458556.9. Ordinary silicate cement, sand, water, polypropylene fiber, latex powder, cellulose ether, wood fiber, expansion agent, water reducer, stabilizer, defoamer, gypsum, modified steel slag powder and composite nano-powder modified glass fiber and other raw materials are used to prepare self-leveling mortar. The product can maintain excellent performance at different temperatures. In order to solve the problem of poor stability of steel slag, the steel slag powder is first neutralized with lauric acid, oxalic acid, and ethylenediaminetetraacetic acid to neutralize the MgO in the steel slag, and then ball-milled to a specific surface area of ​​250-300 for the steel slag powder, and then the ground steel slag powder, silane, ethanol and water are mixed, and the modified steel slag powder is obtained by filtering and drying, but this method is relatively cumbersome. The invention patent is named "A cushion self-leveling glue powder premix and cushion self-leveling mortar based on it", application number CN202011162883.8, which is made of quick-hardening cement, gypsum, redispersible latex powder, water reducer, defoamer, plasticizer, low-viscosity cellulose, and retarder in a suitable ratio. When the cushion self-leveling glue powder premix is ​​used to prepare the cushion self-leveling mortar, it only needs to be mixed with local silicate cement, washed river sand, and heavy calcium powder with water, which is easier to use. However, the use of sulphoaluminate cement as the cementitious material makes the mortar have poor wear resistance.

[0004] In order to meet the special requirements of low shrinkage and wear resistance of self-leveling mortar, the present invention prepares a crack-resistant and wear-resistant self-leveling mortar by studying the formulation system of silicate cement-based self-leveling materials. Summary of the invention

[0005] The purpose of the present invention is to provide a highly crack-resistant and wear-resistant self-leveling mortar, which is prepared by using crack-resistant high-strength cement clinker, auxiliary cementitious materials, heavy calcium powder, modified steel slag powder, gypsum, quartz sand, redispersible latex powder, powdered polycarboxylic acid water reducer, cellulose ether, defoaming agent and water to improve the crack resistance and wear resistance of the self-leveling mortar.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] A highly crack-resistant and wear-resistant self-leveling mortar, comprising the following raw materials in percentage by weight:

[0008] Anti-cracking silicate cement clinker: 15-25wt%;

[0009] Auxiliary gelling material: 5-10wt%;

[0010] Gypsum: 3-7wt%;

[0011] Heavy calcium powder: 5-10wt%

[0012] Modified steel slag powder: 3-7wt%

[0013] 40-70 mesh quartz sand: 30-35wt%;

[0014] 70-120 mesh quartz sand: 20-25wt%;

[0015] And the following auxiliary materials in percentage by weight of the total raw materials:

[0016] Redispersible latex powder: 0.1-0.8wt%;

[0017] Powdered polycarboxylate water reducer: 0.2-0.4wt%;

[0018] Cellulose ether: 0.01-0.02wt%;

[0019] Defoaming agent: 0.1wt%.

[0020] Furthermore, the mineral composition of the crack-resistant silicate cement clinker includes: C3S: 60-68wt%; C2S: 10-15wt%; C3A: 2-5wt%; C4AF: 17-23wt%.

[0021] Furthermore, when the crack-resistant silicate cement clinker is calcined, 3-5wt% of steel slag and 0.1-0.4wt% of CaHPO4 are added to the calcined raw material as additives to promote the burning of C3S in the cement clinker.

[0022] Furthermore, the crack-resistant silicate cement clinker is ground to a specific surface area of ​​320 to 350 m 2 / kg.

[0023] Furthermore, the preparation method of the auxiliary gelling material comprises the following operations:

[0024] (1) naturally air-drying the solid waste to form a mud cake; preferably, the solid waste includes river sludge, papermaking sludge and water treatment sludge;

[0025] (2) placing the mud cake in a muffle furnace, heating it to a target temperature, keeping it warm, and then cooling it down; preferably, the heating rate is 10°C / min, the target temperature is 750-800°C, the holding time is 45min, and the cooling down is rapid air cooling;

[0026] (3) Add 1-2 wt% of polyvinyl alcohol to the cooled mud cake, and grind it to a specific surface area of ​​380-450 m 2 / kg of powder to obtain the auxiliary gelling material.

[0027] Furthermore, the gypsum is dihydrate gypsum or hemihydrate gypsum.

[0028] Furthermore, the fineness of the heavy calcium powder is 400 mesh.

[0029] Furthermore, the preparation method of the modified steel slag powder comprises the following operations:

[0030] (1) Grind the steel slag to a specific surface area of ​​200-250m 2 / kg, add 10-15wt% of water to the slag, and use a granulator to produce 5-10mm slag particles;

[0031] (2) placing the steel slag particles in an autoclave for autoclaving, keeping the temperature, and then cooling down; preferably, the autoclave conditions are: the temperature inside the autoclave is raised to 180° C. for 2 h, the steam pressure is 1.0 MPa, and the temperature is lowered after keeping the temperature for 8 h;

[0032] (3) Dry the steamed steel slag particles to constant weight and grind them to a specific surface area of ​​200-250m 2 / kg, to obtain the modified steel slag powder.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. When crack-resistant silicate cement clinker is calcined, the high KH value of cement clinker is prone to poor burnability. The present invention adopts steel slag and CaHPO4 co-addition, which can significantly reduce the content of f-CaO in cement clinker, improve the metastabilization degree of alite crystals, and thus improve the early strength of clinker. Increasing the C3S content in cement clinker can make cement hydration rapid, increase the amount of bound water in mortar, reduce water evaporation relatively, develop early strength quickly, and shrink small.

[0035] 2. The discharge of solid wastes such as river sludge, papermaking sludge and water treatment sludge is large, which pollutes the environment. The present invention calcines the solid waste at low temperature and quenches it. The calcined solid waste contains a large amount of active ingredients SiO2 and Al2O3, showing high volcanic ash activity, so that the auxiliary cementitious material can react with Ca(OH)2 generated by cement hydration to generate C2ASH8, C3AH6, C4AH 13 and CSH gel, making the self-leveling mortar denser; at the same time, in the presence of gypsum, the generated C3AH6 continues to react to form an expansive hydration product AFt to compensate for the shrinkage of the mortar. In addition, the auxiliary cementitious material has a lamellar structure and can be used as a water retaining agent to store part of the water, reducing the evaporation of water in the self-leveling mortar and thus reducing shrinkage.

[0036] 3. The auxiliary cementitious material of the present invention contains hydrophilic polyvinyl alcohol, which can accelerate the reaction of the auxiliary cementitious material with Ca(OH)2 produced by cement hydration on the one hand; on the other hand, it can increase the cohesion of the mortar, improve workability, and improve the plastic shrinkage of the mortar.

[0037] 4. In addition to the physical effects of filling, nucleation and dilution in the self-leveling mortar, the heavy calcium powder of the present invention also has a chemical effect. It can react with C3A in cement clinker to form carbon aluminate, increase the volume of hydration products, inhibit the conversion of AFt to AFm, and increase the volume stability of the self-leveling mortar. In addition, since the content of C3A in cement clinker is limited, the aluminum content of the system can be increased by adding auxiliary cementitious materials calcined from solid waste, which can strengthen the formation effect of calcium carbon aluminate in the system and further reduce shrinkage.

[0038] 5. The present invention grinds the steel slag into fine particles, adds water to form particles, and hydrates the expansive minerals such as periclase and free calcium oxide in the slag by steam pressing, such as hydrating MgO in the steel slag particles into Mg(OH)2, thereby eliminating its volume instability. During the steam pressing process, the steel slag particles expand and crack, thereby reducing the energy consumption of secondary grinding. After adding modified steel slag powder, the wear resistance of self-leveling mortar can be improved. In addition, the modified steel slag is rich in Mg(OH)2 and Ca(OH)2, which can chemically react with auxiliary cementitious materials in the presence of gypsum to generate AFt and magnesium-containing hydrated calcium silicate, thereby improving the density of cement paste and increasing wear resistance. DETAILED DESCRIPTION

[0039] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0040] Example 1

[0041] As a preferred embodiment of the present invention, a highly crack-resistant and wear-resistant self-leveling mortar provided in this embodiment includes the following raw materials in weight percentage:

[0042] Anti-cracking Portland cement clinker: 15wt%;

[0043] Auxiliary gelling material: 10wt%;

[0044] Gypsum dihydrate: 3wt%;

[0045] 400 mesh heavy calcium powder: 10wt%;

[0046] Modified steel slag powder: 7wt%;

[0047] 40~70 mesh quartz sand: 30wt%;

[0048] 70-120 mesh quartz sand: 25wt%.

[0049] And the following auxiliary materials in percentage by weight of the total raw materials:

[0050] Redispersible latex powder: 0.4wt%;

[0051] Powdered polycarboxylate water reducer: 0.4wt%;

[0052] Cellulose ether: 0.02wt%;

[0053] Defoaming agent: 0.1wt%.

[0054] In this embodiment, the mineral composition of the crack-resistant silicate cement clinker includes: C3S: 68wt%; C2S: 10wt%; C3A: 5wt%; C4AF: 17wt%, and the specific surface area of ​​the crack-resistant silicate cement clinker is 320m 2 / kg.

[0055] When the crack-resistant silicate cement clinker is calcined, 5wt% of steel slag and 0.1wt% of CaHPO4 are added to the calcined raw material as additives to promote the burning of C3S in the cement clinker.

[0056] In this embodiment, the preparation method of the auxiliary gelling material includes the following operations:

[0057] (1) Air-drying the water treatment sludge to form a mud cake;

[0058] (2) placing the mud cake in a muffle furnace, heating it to 750°C at a heating rate of 10°C / min and keeping it at that temperature for 45 min, and then cooling it by rapid air cooling;

[0059] (3) Add 2 wt% polyvinyl alcohol to the cooled mud cake and grind it to a specific surface area of ​​450 m 2 / kg of powder to obtain auxiliary gelling material.

[0060] In this embodiment, the preparation method of modified steel slag powder includes the following operations:

[0061] (1) Grind the steel slag to a specific surface area of ​​250m 2 / kg, add 15wt% of water to the slag, and use a granulator to produce 5-10mm slag particles;

[0062] (2) The particles were placed in an autoclave, the temperature inside the autoclave was raised to 180°C for 2 hours, the steam pressure was 1.0 MPa, and the temperature was lowered after keeping the temperature for 8 hours.

[0063] (3) The autoclaved slag particles are dried to constant weight and then ground to a specific surface area of ​​235 m 2 / kg, and modified steel slag powder is obtained.

[0064] Example 2

[0065] As a preferred embodiment of the present invention, a highly crack-resistant and wear-resistant self-leveling mortar provided in this embodiment includes the following raw materials in weight percentage:

[0066] Anti-cracking Portland cement clinker: 25wt%;

[0067] Auxiliary gelling material: 5wt%;

[0068] Gypsum dihydrate: 7wt%;

[0069] 400 mesh heavy calcium powder: 5wt%;

[0070] Modified steel slag powder: 3wt%;

[0071] 40-70 mesh quartz sand: 35wt%;

[0072] 70~120 mesh quartz sand: 20wt%.

[0073] And the following auxiliary materials in percentage by weight of the total raw materials:

[0074] Redispersible latex powder: 0.8wt%;

[0075] Powdered polycarboxylate water reducer: 0.2wt%;

[0076] Cellulose ether: 0.02wt%;

[0077] Defoaming agent: 0.1wt%.

[0078] In this embodiment, the mineral composition of the crack-resistant silicate cement clinker includes: C3S: 60wt%; C2S: 15wt%; C3A: 2wt%; C4AF: 23wt%, and the specific surface area of ​​the crack-resistant silicate cement clinker is 350m 2 / kg.

[0079] When the crack-resistant silicate cement clinker is calcined, 3wt% of steel slag and 0.4wt% of CaHPO4 are added to the calcined raw material as additives to promote the burning of C3S in the cement clinker.

[0080] In this embodiment, the preparation method of the auxiliary gelling material includes the following operations:

[0081] (1) Air-drying the water treatment sludge to form a mud cake;

[0082] (2) placing the mud cake in a muffle furnace, heating it to 800°C at a heating rate of 10°C / min and keeping it at that temperature for 45 min, and then cooling it by rapid air cooling;

[0083] (3) Add 1 wt% polyvinyl alcohol to the cooled mud cake and grind it to a specific surface area of ​​380 m 2 / kg of powder to obtain auxiliary gelling material.

[0084] In this embodiment, the preparation method of modified steel slag powder includes the following operations:

[0085] (1) Grind the steel slag to a specific surface area of ​​200m 2 / kg, add 10wt% of water to the slag, and use a granulator to produce 5-10mm slag particles;

[0086] (2) The particles were placed in an autoclave, the temperature inside the autoclave was raised to 180°C for 2 hours, the steam pressure was 1.0 MPa, and the temperature was lowered after keeping the temperature for 8 hours.

[0087] (3) The autoclaved slag particles are dried to constant weight and then ground to a specific surface area of ​​250 m 2 / kg, and modified steel slag powder is obtained.

[0088] Example 3

[0089] As a preferred embodiment of the present invention, a highly crack-resistant and wear-resistant self-leveling mortar provided in this embodiment includes the following raw materials in weight percentage:

[0090] Anti-cracking silicate cement clinker: 20wt%;

[0091] Auxiliary cementitious material: 7wt%;

[0092] Gypsum dihydrate: 5wt%;

[0093] 400 mesh heavy calcium powder: 8wt%;

[0094] Modified steel slag powder: 5wt%;

[0095] 40~70 mesh quartz sand: 32wt%;

[0096] 70-120 mesh quartz sand: 23wt%.

[0097] And the following auxiliary materials in percentage by weight of the total raw materials:

[0098] Redispersible latex powder: 0.1wt%;

[0099] Powdered polycarboxylate water reducer: 0.3wt%;

[0100] Cellulose ether: 0.02wt%;

[0101] Defoaming agent: 0.1wt%.

[0102] In this embodiment, the mineral composition of the anti-cracking silicate cement clinker includes: C3S: 64wt%; C2S: 12wt%; C3A: 4wt%; C4AF: 20wt%, and the specific surface area of ​​the anti-cracking silicate cement clinker is 335m 2 / kg.

[0103] When the crack-resistant silicate cement clinker is calcined, 3wt% of steel slag and 0.3wt% of CaHPO4 are added to the calcined raw material as additives to promote the burning of C3S in the cement clinker.

[0104] In this embodiment, the preparation method of the auxiliary gelling material includes the following operations:

[0105] (1) Air-drying the water treatment sludge to form a mud cake;

[0106] (2) placing the mud cake in a muffle furnace, heating it to 800°C at a heating rate of 10°C / min and keeping it at that temperature for 45 min, and then cooling it by rapid air cooling;

[0107] (3) Add 1.5 wt% of polyvinyl alcohol to the cooled mud cake and grind it to a specific surface area of ​​420 m2 / kg of powder to obtain auxiliary gelling material.

[0108] In this embodiment, the preparation method of modified steel slag powder includes the following operations:

[0109] (1) Grind the steel slag to a specific surface area of ​​230 m 2 / kg, add 12wt% of water to the slag, and use a granulator to produce 5-10mm slag particles;

[0110] (2) The particles were placed in an autoclave, the temperature inside the autoclave was raised to 180°C for 2 hours, the steam pressure was 1.0 MPa, and the temperature was lowered after keeping the temperature for 8 hours.

[0111] (3) The autoclaved slag particles are dried to constant weight and then ground to a specific surface area of ​​220 m 2 / kg, and modified steel slag powder is obtained.

[0112] Comparative Example 1

[0113] The self-leveling mortar of this comparative example is the same as that of Example 1, except that steel slag and CaHPO4 are not added during the calcination of the silicate cement clinker.

[0114] Comparative Example 2

[0115] The self-leveling mortar of this comparative example is the same as that of Example 1 except that the auxiliary cementitious material is not included and the anti-cracking silicate cement clinker is 30wt%.

[0116] Comparative Example 3

[0117] The self-leveling mortar of this comparative example is the same as that of Example 1 except that ordinary steel slag powder is used instead of modified steel slag powder.

[0118] The self-leveling mortars prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were tested for basic physical and mechanical properties, shrinkage and wear resistance. The test results are shown in Table 1.

[0119] Table 1 Basic physical and mechanical properties of self-leveling mortar

[0120]

[0121]

[0122] The sample preparation and general performance testing of the self-leveling mortar prepared in the embodiments of the present invention and the comparative examples were carried out in accordance with JC / T985-2017 "cement-based self-leveling mortar for floor use".

[0123] As can be seen from Table 1, the self-leveling mortar prepared in the embodiment of the present invention has fluidity, mechanical properties, dimensional change rate and wear resistance that meet the requirements of the specification, and has excellent wear resistance and dimensional stability.

[0124] As can be seen from Table 1, in Comparative Example 1, no steel slag and CaHPO4 were added during the clinker calcination process, resulting in f-CaO exceeding 2.0wt% in the cement clinker. Compared with Example 1, the mortar fluidity was small, the dimensional change rate exceeded the specification requirements, and the 28d strength was low. In Comparative Example 2, no auxiliary cementitious material was added. Compared with Example 2, due to the lack of auxiliary cementitious materials with a large water requirement, the mortar fluidity increased and the 1d strength increased, but the aluminum content in the system decreased, resulting in a -0.13% shrinkage of the mortar, and a lack of volcanic ash reaction, resulting in low strength in the later stage. In Comparative Example 3, steel slag was used instead of modified steel slag. Since the steel slag contained periclase and free calcium oxide, the mortar volume expanded, the 28d strength decreased, and cracking occurred.

[0125] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solutions of the present invention, rather than limiting them, and certainly not limiting the patent scope of the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In other words, any changes or modifications made to the main design concept and spirit of the present invention that have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention. In addition, the direct or indirect application of the technical solutions of the present invention in other related technical fields is also included in the patent protection scope of the present invention.

Claims

1. A highly crack-resistant and wear-resistant self-leveling mortar, characterized in that: The raw materials include the following weight percentages: Anti-cracking silicate cement clinker: 15-25wt%; Auxiliary gelling material: 5-10wt%; Gypsum: 3-7wt%; Heavy calcium powder: 5-10wt% Modified steel slag powder: 3-7wt% 40-70 mesh quartz sand: 30-35wt%; 70-120 mesh quartz sand: 20-25wt%; And the following auxiliary materials in percentage by weight of the total raw materials: Redispersible latex powder: 0.1-0.8wt%; Powdered polycarboxylate water reducer: 0.2-0.4wt%; Cellulose ether: 0.01-0.02wt%; Defoaming agent: 0.1wt%.

2. A highly crack-resistant and wear-resistant self-leveling mortar according to claim 1, characterized in that: The mineral composition of the anti-cracking silicate cement clinker includes: C3S: 60-68wt%; C2S: 10-15wt%; C3A: 2-5wt%; C4AF: 17-23wt%.

3. The highly crack-resistant and wear-resistant self-leveling mortar according to claim 1, characterized in that: When the crack-resistant silicate cement clinker is calcined, 3-5wt% of steel slag and 0.1-0.4wt% of CaHPO4 are added to the calcined raw material as additives to promote the burning of C3S in the cement clinker.

4. The highly crack-resistant and wear-resistant self-leveling mortar according to claim 1, characterized in that: The anti-cracking silicate cement clinker is ground to a specific surface area of ​​320 to 350 m 2 / kg.

5. The highly crack-resistant and wear-resistant self-leveling mortar according to claim 1, characterized in that: The preparation method of the auxiliary gelling material comprises the following operations: (1) naturally air-drying the solid waste to form a mud cake; preferably, the solid waste includes river sludge, papermaking sludge and water treatment sludge; (2) placing the mud cake in a muffle furnace, heating it to a target temperature, keeping it warm, and then cooling it down; preferably, the heating rate is 10°C / min, the target temperature is 750-800°C, the holding time is 45min, and the cooling down is rapid air cooling; (3) Add 1-2 wt% of polyvinyl alcohol to the cooled mud cake, and grind it to a specific surface area of ​​380-450 m 2 / kg of powder to obtain the auxiliary gelling material.

6. The highly crack-resistant and wear-resistant self-leveling mortar according to claim 1, characterized in that: The gypsum is dihydrate gypsum or hemihydrate gypsum.

7. The highly crack-resistant and wear-resistant self-leveling mortar according to claim 1, characterized in that: The fineness of the heavy calcium powder is 400 meshes.

8. The highly crack-resistant and wear-resistant self-leveling mortar according to claim 1, characterized in that: The preparation method of the modified steel slag powder comprises the following operations: (1) Grind the steel slag to a specific surface area of ​​200-250m 2 / kg, add 10-15wt% of water to the slag, and use a granulator to produce 5-10mm slag particles; (2) placing the steel slag particles in an autoclave for autoclaving, keeping the temperature, and then cooling down; preferably, the autoclave conditions are: the temperature inside the autoclave is raised to 180° C. for 2 h, the steam pressure is 1.0 MPa, and the temperature is lowered after keeping the temperature for 8 h; (3) Dry the steamed steel slag particles to constant weight and grind them to a specific surface area of ​​200-250m 2 / kg, to obtain the modified steel slag powder.

Citation Information

Patent Citations

  • Autoclaving treatment modification technology for converter steel slag and applications thereof

    CN103571983A

  • Self-leveling mortar and preparation method thereof

    CN108059429A