Silica fume modified double-liquid grouting material and preparation method thereof

By introducing silicon fume and water reducing agent into cement water glass double-liquid grouting material, silicon fume modified double-liquid grouting material is prepared, which solves the problem of long settling time and poor stability of traditional grouting materials in water-rich formations. , achieves high strength and good water dissolution resistance, and is suitable for formation reinforcement and leakage plugging in water-rich karst environments.

CN118993686APending Publication Date: 2024-11-22WENSHAN UNIV

Patent Information

Application Number
CN202411125194.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional single-liquid grouting materials and double-liquid grouting materials have problems such as uncontrollable settling time, poor slurry stability, weak late-stage strength of stone bodies, and insufficient water dissolution and impermeability resistance in water-rich formation environments.

Method used

Using silicon fume modified double-liquid grouting material, by introducing silicon fume and water reducing agent into cement water glass double-liquid grouting material, the optimal ratio is determined through orthogonal experiments, and the settling time is adjustable and the stability is good. grouting materials improve mechanical properties and durability.

Benefits of technology

It has achieved high strength, water dissolution resistance and excellent permeability of the slurry stone body, and has good green and environmental protection and stability. It is suitable for leak plugging and reinforcement of water-rich karst environmental formations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993686A_ABST
    Figure CN118993686A_ABST
Patent Text Reader

Abstract

The invention discloses a silica fume modified double-liquid grouting material which comprises a liquid A and a liquid B. The volume ratio of the liquid A to the liquid B is 1: 1-2.5: 1. The silica fume modified double-liquid grouting material comprises the following raw materials: ordinary Portland cement, water, water glass, silica fume and a water reducing agent. According to the silica fume modified double-liquid grouting material and the preparation method thereof, a certain amount of silica fume and a water reducing agent are introduced on the basis of a cement and water glass double-liquid grouting material to modify the cement and water glass double-liquid grouting material, an orthogonal experiment is carried out in combination with related influence factors of basic characteristics of grout to obtain a better proportion, and the silica fume modified double-liquid grouting material is prepared; therefore, the silica fume modified double-liquid grouting material has excellent mechanical properties and durability, the optimal mix proportion is determined through an orthogonal experiment and a trend chart of each factor on evaluation indexes, and the feasibility of the silica fume modified double-liquid grouting material is analyzed from a theoretical level. Therefore, the grouting material has the advantages of being environmentally friendly, good in stability, controllable in setting time, high in slurry stone body strength in different maintenance stages, and excellent in water corrosion resistance and impermeability, and has a good anti-seepage and leaking stoppage effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of grouting materials, in particular to a silica fume modified double-liquid grouting material and a preparation method thereof. Background Art

[0002] In recent years, my country has made rapid progress in the construction of tunnels and underground projects. However, my country has a vast territory and a complex engineering hydrogeological environment. Some engineering construction involves water-rich strata, which are prone to geological disasters. The environment of water-rich strata is extremely unstable, often accompanied by geological characteristics such as dynamic and static water, pores and filling bodies. Since water-rich strata have the characteristics of uneven stress, poor rock cementation and strong impact of flowing water, improper treatment can easily induce secondary geological disasters such as sudden water inrush, surface subsidence and drying up of surface water. Among them, the problem of sudden water inrush is particularly prominent, causing huge economic losses and seriously affecting construction efficiency. Therefore, the hidden dangers of sudden water inrush have been widely valued in the construction of tunnels and underground projects. It not only affects the construction progress, but also poses a danger to the safety and stability of the building. It is also a major technical problem restricting the construction of tunnels and underground projects.

[0003] Grouting technology is a commonly used technical means in engineering construction. It prepares cementitious materials into slurry in proportion, injects it into the cracks of rock formations with the help of pressure equipment, and bonds with the rock and soil to form a stone body after solidification, thereby improving the compressive strength and anti-permeability of the rock formation, reducing the porosity, enhancing the physical and mechanical properties of the rock and soil and the overall stability of the rock formation, and ultimately achieving the purpose of strengthening the rock formation, improving the anti-seepage, waterproof and water-blocking properties. It can effectively prevent the occurrence of geological disasters in engineering construction. However, with the in-depth advancement of underground projects, the water-rich stratum environment faced is also more severe. When using traditional grouting materials for treatment, engineering construction is often hindered due to substandard material performance.

[0004] There are many grouting materials commonly used in the grouting construction process of underground projects. Traditional single-liquid grouting materials have the advantages of wide sources, low prices, green environmental protection, and simple grouting process. However, it is undeniable that traditional single-liquid grouting materials have problems such as long setting time, poor water flow erosion resistance, slow growth of slurry stone body strength, and low stone rate, which cannot effectively meet the requirements of anti-seepage and reinforcement management of water-rich strata. Chemical grouting materials have also been developed and applied, with advantages such as low viscosity, short setting time, and easy volume expansion, but they also have disadvantages such as poor durability of slurry stone body, low strength, expensive raw materials, violent slurry reaction, and easy environmental pollution. Cement-water glass two-liquid grouting materials have the advantages of short setting time, high slurry solubility, and high stone rate, and are widely used in grouting, water-stopping, and reinforcement of tunnels and underground projects. However, there are also disadvantages. The setting time and stability of cement-water glass two-liquid grouting materials are easily affected by factors such as water-cement ratio and volume ratio, and will affect the change of the later strength of the slurry stone body and the poor durability.

[0005] Therefore, we proposed a silica fume modified double liquid grouting material and a preparation method thereof in order to solve the above-mentioned problems. Summary of the invention

[0006] The purpose of the present invention is to provide a silica fume modified two-liquid grouting material and a preparation method thereof, so as to solve the problems of uncontrollable setting time, poor slurry stability, weak late strength of the stone body, and insufficient water dissolution resistance and anti-seepage performance of the existing traditional single-liquid grouting materials and traditional two-liquid grouting materials proposed in the above background technology.

[0007] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a silica fume modified two-liquid grouting material, comprising liquid A and liquid B, wherein the volume ratio of liquid A to liquid B is 1:1 to 2.5:1, and the raw materials include: ordinary Portland cement, water, water glass, silica fume, and a water reducer.

[0008] Preferably, liquid A includes the following components in parts by mass: 250-400 parts of ordinary Portland cement, 7.5-30 parts of silica fume, 1.0-3.25 parts of water reducer, and 150-200 parts of water (silica fume accounts for 3%-12%; water reducer 0.4%-1.3%; water-cement ratio 0.6-1.2; volume ratio 1:1-2.5:1).

[0009] Preferably, liquid B comprises the following components in parts by mass: 245 to 370 parts of water glass.

[0010] Preferably, the water glass is liquid sodium silicate water glass with a modulus of 3.03 to 3.3 and a Baume degree of 38.5 to 41.5°Bé.

[0011] Preferably, the silica fume has a silicon dioxide content of 98% and a particle size of 2.6 microns.

[0012] Preferably, the water reducer is a polycarboxylic acid high-efficiency water reducer.

[0013] Preferably, ordinary Portland cement, water, silica fume and water reducing agent are uniformly mixed, wherein the water-cement ratio is 0.6-1.2, and liquid A and liquid B are mixed at a volume ratio of 1:1-2.5:1 to obtain a silica fume modified two-liquid grouting material.

[0014] A method for preparing a silica fume modified double-liquid grouting material comprises the following steps:

[0015] Step 1: The factors that affect the basic properties of the two-liquid grouting material are: water-cement ratio, volume ratio, silica fume dosage, and water-reducing agent dosage; the experience level range of each factor is determined by relevant engineering experience and published results, and then the level of each factor in the orthogonal experimental scheme is determined; the orthogonal experimental scheme is to conduct an orthogonal combination design of the factors and the corresponding level numbers selected to determine the specific experimental scheme;

[0016] Step 2: The basic properties of the two-liquid grouting material (setting time, water separation rate, stone rate and compressive strength) were tested by referring to the standards JGJT21110 "Technical Specifications for Cement-Water Glass Two-Liquid Grouting in Construction Engineering", DL / T5150-2001 "Testing Procedures for Hydraulic Concrete", and GB / T 50081 "Standard for Test Methods for Physical and Mechanical Properties of Concrete";

[0017] Step 3: The trend graph is a relationship graph between different levels of each factor and the evaluation index, including positive correlation and negative correlation trend graphs: the horizontal axis of the trend graph is the different levels of the research factor, and the vertical axis is the evaluation index;

[0018] The extreme value of each factor level is used as the evaluation index of the degree of influence. The change rate of material performance is obtained after the basic characteristics test of double-liquid grouting material is designed by orthogonal experimental method. After processing the orthogonal experimental data results, the significant level of the influence of each factor on the basic performance of the slurry is found and the optimal ratio is obtained as 12% silica fume, 0.8 water-cement ratio, 1.5:1 volume ratio, and 1.0% water reducer.

[0019] Step 4: The water-cement ratio of the traditional single-liquid grouting material is the same as the water-cement ratio of the silica fume modified two-liquid grouting material with the optimal ratio obtained by orthogonal experiment, and the water-cement ratio and volume ratio of the traditional two-liquid grouting material are also the same;

[0020] The mechanical properties and durability of silica fume modified two-liquid grouting materials with optimal ratios are compared with those of traditional single-liquid grouting materials and traditional two-liquid grouting materials, specifically the comparison of compressive strength, water corrosion resistance and impermeability under different curing environments and ages, with reference to GB / T 50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete".

[0021] Compared with the prior art, the beneficial effects of the present invention are as follows: the silica fume modified double liquid grouting material and the preparation method thereof adopt a new structural design, and the specific contents thereof are as follows:

[0022] 1. A certain amount of silica fume and water reducer are introduced into the cement-water glass two-liquid grouting material to modify it. An orthogonal experiment is conducted on the relevant influencing factors of the basic properties of the slurry to obtain a better ratio, and a silica fume modified two-liquid grouting material is prepared. Compared with traditional single-liquid grouting materials and two-liquid grouting materials, it has excellent mechanical properties and durability;

[0023] 2. Water-cement ratio, volume ratio, silica fume dosage and water reducing agent dosage are the relevant factors that affect the basic properties of slurry. Orthogonal analysis of these factors is highly targeted. The level range of each factor is determined by engineering experience and published results, making the parameter values ​​more scientific and reasonable.

[0024] 3. Analyzing based on the orthogonal experimental results and the extreme values ​​of each factor can better reflect the true relationship of the effects of each factor on the basic properties of the slurry, making the research results more reliable;

[0025] 4. The positive correlation trend graph can directly reflect the influence of different levels of a certain factor on the evaluation index, and the negative correlation trend graph can directly reflect the influence of different factors on a certain evaluation index;

[0026] 5. Based on the existing cement and water glass slurry mixed with a certain proportion of silica fume and water reducing agent, a grouting material with adjustable setting time, good stability, excellent mechanical properties and durability is formulated. The optimal mix ratio is determined through orthogonal experiments and trend diagrams of various factors on evaluation indicators. The feasibility of silica fume modified double-liquid grouting materials is analyzed from a theoretical level. Compared with traditional single-liquid grouting materials and traditional double-liquid grouting materials, it has the advantages of being green and environmentally friendly, good stability, controllable setting time, high strength of slurry stone body at different maintenance stages, excellent resistance to water dissolution and impermeability, and has good anti-seepage and plugging effect. It has broad application prospects in water-rich karst environment strata. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a schematic diagram of the preparation process of the present invention;

[0028] Figure 2 This is a comparison chart of the water separation rate and stone formation rate of the grouting materials of Examples 1-3 of the present invention;

[0029] Figure 3 This is a comparison chart of the setting time of the grouting materials of Examples 1-3 of the present invention;

[0030] Figure 4 A comparison chart of the compressive strength of the grouting materials of Examples 1-3 of the present invention at different curing ages;

[0031] Figure 5 This is a comparison chart of the water corrosion resistance of the grouting materials of Examples 1-3 of the present invention after 3 days of curing;

[0032] Figure 6 This is a comparison chart of the water corrosion resistance of the grouting materials of Examples 1-3 of the present invention after curing for 7 days;

[0033] Figure 7 This is a comparison chart of the water corrosion resistance of the grouting materials of Examples 1-3 of the present invention after curing for 28 days;

[0034] Figure 8 It is a comparison chart of the anti-seepage performance of the grouting materials of Examples 1-3 of the present invention. DETAILED DESCRIPTION

[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Embodiment 1

[0037] A silica fume modified two-liquid grouting material comprises the following components in parts by mass:

[0038] Liquid A comprises the following components by mass: 250-400 parts of ordinary Portland cement, 7.5-30 parts of silica fume, 1.0-3.25 parts of water reducer, and 150-200 parts of water (3%-12% of silica fume; 0.4%-1.3% of water reducer; 0.6-1.2 of water-cement ratio; and 1:1-2.5:1 of volume ratio), wherein the silica fume has a silicon dioxide content of 98% and a particle size of 2.6 microns, and the water reducer is a polycarboxylic acid high-efficiency water reducer;

[0039] The components of liquid B by mass are: 245 to 370 parts of water glass, wherein the water glass is liquid sodium silicate water glass, with a modulus of 3.03 to 3.3 and a Baume degree of 38.5 to 41.5°Bé.

[0040] Embodiment 2

[0041] A silica fume modified two-liquid grouting material comprises the following components in parts by mass:

[0042] Liquid A has the following components by mass: 230-380 parts of ordinary Portland cement, 6.5-25 parts of silica fume, 0.9-2.98 parts of water reducer, and 130-170 parts of water (2.5%-10% of silica fume; 0.3%-1% of water reducer; 0.4-1 water-cement ratio; 0.9:1-2.3:1 volume ratio), wherein the silica fume has a silicon dioxide content of 97.8% and a particle size of 2.4 microns, and the water reducer is a polycarboxylic acid high-efficiency water reducer;

[0043] The components of liquid B by mass are: 225-350 parts of water glass, wherein the water glass is liquid sodium silicate water glass, with a modulus of 3.02-3.25 and a Baume degree of 37.5-40.5°Bé.

[0044] Embodiment 3

[0045] A silica fume modified two-liquid grouting material comprises the following components in parts by mass:

[0046] Liquid A has the following components by mass: 240-350 parts of ordinary Portland cement, 6-23 parts of silica fume, 0.6-2.60 parts of water reducer, and 140-190 parts of water (2.2%-11.5% of silica fume; 0.25%-0.87% of water reducer; 0.25-0.9 of water-cement ratio; 0.7:1-2:1 of volume ratio), wherein the silica fume has a silicon dioxide content of 96% and a particle size of 2.2 microns, and the water reducer is a polycarboxylic acid high-efficiency water reducer;

[0047] The components of liquid B in terms of mass fractions are: 210 to 320 parts of water glass, wherein the water glass is liquid sodium silicate water glass, with a modulus of 3 to 3.1 and a Baume degree of 36.4 to 39.45°Bé.

[0048] The present invention provides a method for preparing a silica fume modified double-liquid grouting material, comprising the following steps:

[0049] S1. Add silica fume, silicate cement and water reducing agent into water and stir evenly to obtain liquid A;

[0050] S2, using water glass as liquid B;

[0051] S3. Evenly mix liquid A and liquid B in a volume ratio of 1:1 to 2.5:1 to obtain the silica fume modified two-liquid grouting material.

[0052] The following is combined with Figure 1-Figure 8 The present invention is further described in Example 1 to Example 3. The present invention is based on evaluating the influence of different factors on the basic properties of the double liquid grouting material, combining various factors to design orthogonal experiments at different levels, comprehensively studying various factors, and obtaining a better ratio. Then, a silica fume modified double liquid grouting material is prepared, and the mechanical properties and durability properties are compared with those of the traditional single liquid grouting material and the traditional double liquid grouting material, comprising the following steps:

[0053] Step 1: Determine the factors that affect the basic properties of the dual-liquid grouting material, and design an orthogonal experimental scheme based on the experience level of each factor;

[0054] Step 2: According to the orthogonal experimental scheme, basic characteristics research tests such as slurry coagulation time, water separation rate, stone rate and changes in compressive strength of slurry stone body during different curing ages were carried out;

[0055] Step 3: Draw a trend chart based on the measured experimental data and conduct an intuitive analysis of each influencing factor;

[0056] Step 4: Find the factors that have a significant impact on the basic properties of the dual-liquid grouting material through orthogonal experimental data processing;

[0057] Step 5: Combine the trend chart of the test data of each factor and the optimal factor level to obtain a better ratio and prepare the silica fume modified double liquid grouting material;

[0058] Step 6: Compare the mechanical properties and durability of the silica fume modified two-liquid grouting material with the optimal ratio with the traditional single-liquid grouting material and the traditional two-liquid grouting material.

[0059] In step 1, the influencing factors affecting the basic properties of the dual-liquid grouting material are determined, and an orthogonal experimental scheme is designed according to the experience level of each factor. The process is to take the water-cement ratio, volume ratio, silica fume content, water-reducing agent content, etc. as relevant factors affecting the basic properties of the slurry, and determine the approximate range of the level of each factor based on engineering experience and published related results, so as to determine the level of each factor required for the test scheme, and design the experiment according to the level of each factor. For example, AiBjCkDl represents an experimental scheme with the combination of the i-th level of factor A, the j-th level of factor B, the k-th level of factor C, and the l-th level of factor D.

[0060] In the study of the basic properties of the slurry in step 2, the slurry was prepared as follows:

[0061] (1) Preparation of Liquid A: Mix ordinary Portland cement, water, silica fume and water reducing agent evenly, wherein the water-cement ratio is 0.6-1.2;

[0062] (2) Liquid A and liquid B are mixed in a volume ratio of 1:1-2.5:1 to obtain a silica fume modified two-liquid grouting material.

[0063] Measurement of setting time in the study of basic properties of slurries by orthogonal experimental scheme in step 2:

[0064] By designing a four-factor four-level orthogonal test plan, the water-cement ratio of 0.6-1.2, the volume ratio of 1:1-2.5:1, the silica fume content of 3%-12%, and the water reducer content of 0.4%-1.3% were selected for orthogonal experimental design. According to the specific test specifications, the "inverted cup method" was used for testing. Liquid A and liquid B were mixed evenly, and the cup was quickly inverted to observe the solidification of the slurry. When the slurry does not flow in the cup, it is the gel time. Repeat the measurement twice and take the average.

[0065] In the orthogonal experimental scheme in step 2, the water separation rate and stone formation rate were measured by designing a four-factor four-level orthogonal experimental scheme. The water-cement ratio of 0.6-1.2, the volume ratio of 1:1-2.5:1, the silica fume content of 3%-12%, and the water reducer content of 0.4%-1.3% were selected to prepare the slurry. According to the specific test specifications, liquid A and liquid B were mixed evenly, poured into a measuring cylinder with a range of 250ml to measure 200ml of slurry, recorded as the initial volume of the slurry V1; after standing for 2h, the volume of precipitated water was recorded as V2, and the ratio of V2 to V1 was the water separation rate of the slurry. The measurement was repeated twice and the average was taken. The stone formation rate was measured as follows: the ratio of the slurry consolidation body volume V3 to V1 was the slurry stone formation rate.

[0066] In the study of the basic characteristics of the slurry conducted by the orthogonal experimental scheme in step 2, the changes in the compressive strength of the slurry stone body at different curing ages were studied by designing a four-factor four-level orthogonal experimental scheme. The water-cement ratio of 0.6-1.2, the volume ratio of 1:1-2.5:1, the silica fume content of 3%-12%, and the water reducer content of 0.4%-1.3% were selected to prepare the slurry. According to the specific test specifications, liquid A and liquid B were evenly mixed and poured into a columnar test mold with a height of 10 cm and a diameter of 6 cm. After curing for 1 day, the mold was removed and placed in a standard curing box for curing for 3d, 7d, and 28d for indoor uniaxial compressive strength test. Each group was tested 3 times and the average value was taken.

[0067] The trend chart in step 3 is a relationship chart between different levels of each factor and the evaluation index, including a positive trend chart and a negative trend chart. The horizontal axis of the positive trend chart represents the different levels of the studied factor, and its vertical axis represents the evaluation index. The horizontal axis of the negative trend chart represents the evaluation index, and the vertical axis represents the different levels of the factor. Both trend charts can be set to double vertical axes or more to intuitively compare the degree of influence of different levels of each factor on the same evaluation index.

[0068] In step 4, the orthogonal experimental data are processed to find the factors that have a significant effect on the basic characteristics of the slurry, and the range analysis value of each factor level is used as one of the evaluation criteria for orthogonal experimental data analysis, so as to determine the factor level that has a significant effect on the basic characteristics.

[0069] In step 5, the optimal level combination of each influencing factor is determined based on the range analysis value of each factor level and the trend chart of the effect on slurry performance, which is a water-cement ratio of 0.8, a volume ratio of 1.5:1, a silica fume content of 12%, and a water reducer content of 1.0%, and the silica fume modified two-liquid grouting material is prepared with the optimal ratio.

[0070] In step 6, the silica fume modified two-liquid grouting material with the optimal ratio is compared with the traditional single-liquid grouting material and the traditional two-liquid grouting material in terms of mechanical properties and durability such as water corrosion resistance and impermeability in accordance with relevant test specifications.

[0071] The specific experimental steps are as follows:

[0072] According to step 5, the optimal level combination of the influencing factors on the basic properties of the slurry is a water-cement ratio of 0.8, a volume ratio of 1.5:1, a silica fume content of 12%, and a water reducer content of 1.0% to prepare the silica fume modified two-liquid grouting material.

[0073] The proportion of the traditional single-liquid grouting material in step 6 is to control the water-cement ratio to 0.8, so that it is the same as the water-cement ratio of the silica fume modified two-liquid grouting material under the optimal proportion.

[0074] The proportion of the traditional two-liquid grouting material in step 6 is to control the water-cement ratio to 0.8 and the volume ratio to 1.5:1, so that the water-cement ratio and volume ratio are the same as those of the silica fume modified two-liquid grouting material under the optimal proportion.

[0075] In step 6, the mechanical properties of the silica fume modified two-liquid grouting material are compared with those of the traditional single-liquid grouting material and the traditional two-liquid grouting material. The slurry is prepared according to the slurry proportions in steps (1), (2), and (3), and then the slurry is poured into a test mold and cured for 1 day before demolding. The compressive strength test is then performed after curing for 3 days, 7 days, and 28 days under a standard curing environment.

[0076] In step 6, the comparison of the water corrosion resistance of the silica fume modified two-liquid grouting material with the traditional single-liquid grouting material and the traditional two-liquid grouting material is as follows: the slurry is prepared according to the slurry proportions of steps (1), (2), and (3), and then the slurry is poured into a test mold and cured for 1 day before demolding.

[0077] In the comparative test of the water corrosion resistance of silica fume modified two-liquid grouting material with traditional single-liquid grouting material and traditional two-liquid grouting material in step 6, the test conditions are as follows: fill the water tank with tap water, and place the water pump upside down and horizontally at the bottom of the water tank so that the direction of the water outlet is parallel to the bottom of the water tank.

[0078] In the comparative test of the water corrosion resistance of silica fume modified two-liquid grouting material with traditional single-liquid grouting material and traditional two-liquid grouting material in step 6, the test conditions are as follows: the water tank is connected to the power supply to simulate the underground dynamic water environment, and the dynamic water flow rate is controlled to 0.5m / s by the flow regulating valve.

[0079] In step 6, the comparison of the water corrosion resistance of the silica fume modified two-liquid grouting material with the traditional single-liquid grouting material and the traditional two-liquid grouting material is as follows: the slurry is prepared according to the slurry proportions of steps (1), (2), and (3), the slurry is poured into a test mold and cured for 1 day, then demolded and placed in a water tank, and cured in moving water for 3 days, 7 days, and 28 days before being taken out to test the compressive strength of the stone body.

[0080] In the comparative test of water corrosion resistance of silica fume modified two-liquid grouting material with traditional single-liquid grouting material and traditional two-liquid grouting material in step 6, a control group is set up, and specimens with the same proportion are prepared for standard curing. The curing age is the same as the curing in static water or dynamic water environment. After reaching the specified age, the specimens are taken out and the compressive strength is tested.

[0081] In the comparative test of the water dissolution resistance of the silica fume modified two-liquid grouting material with the traditional single-liquid grouting material and the traditional two-liquid grouting material in step 6, the stone body strength dissolution coefficient is used as the evaluation index of the slurry's water dissolution resistance.

[0082] In step 6, the anti-seepage performance of the silica fume modified two-liquid grouting material is compared with that of the traditional single-liquid grouting material and the traditional two-liquid grouting material. The slurry is prepared according to the slurry proportions of steps (1), (2), and (3), and then the slurry is poured into a Φ70mm×80mm×30mm test mold and cured for 1 day for demoulding.

[0083] In the comparative test of the anti-seepage performance of the silica fume modified two-liquid grouting material with the traditional single-liquid grouting material and the traditional two-liquid grouting material in step 6, the test piece removed from the test mold after curing for 1 day was placed in a curing box for further curing for 2 days.

[0084] In the comparative test of the anti-permeability performance of the silica fume modified two-liquid grouting material with the traditional single-liquid grouting material and the traditional two-liquid grouting material in step 6, the specimens cured in the curing box for 2 days were placed in a water-resistance meter for testing in groups of 6 specimens.

[0085] In the comparative test of the anti-seepage performance of the silica fume modified two-liquid grouting material with the traditional single-liquid grouting material and the traditional two-liquid grouting material in step 6, the stone body placed in the anti-seepage instrument is tested by the "step-by-step pressurization method", and the maximum water seepage pressure is used as the evaluation index of the anti-seepage performance of the slurry.

[0086] Through the above test comparison, it can be known that the present invention solves the shortcomings of most commonly used grouting materials in water-rich environments, such as long setting time, low stone rate, poor volume stability, slow strength growth of slurry stone body and poor durability. In particular, compared with the stone body of traditional double-liquid grouting materials, the present invention has obvious anti-water dissolution and anti-seepage effects, low water separation rate and high stone rate, high later strength, and the materials used are cheap and non-toxic, simple to prepare, without too many additives, and suitable for on-site grouting applications. During use, depending on the amount of water inflow from the formation and the injectability of the rock formation, the amount of silica fume added can be appropriately adjusted on the basis of the optimal matching, and the water-cement ratio and volume ratio can be adjusted in time, so that the slurry has good fluidity, strong stability, controllable setting time, high stone body strength and good anti-seepage performance.

[0087] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A silica fume modified two-liquid grouting material, characterized in that: It includes liquid A and liquid B, the volume ratio of liquid A to liquid B is 1:1 to 2.5:1, and the raw materials include: ordinary Portland cement, water, water glass, silica fume, and water reducing agent.

2. The silica fume modified two-liquid grouting material according to claim 1, characterized in that: Liquid A includes the following components in parts by mass: 250-400 parts of ordinary Portland cement, 7.5-30 parts of silica fume, 1.0-3.25 parts of water reducer, and 150-200 parts of water (silica fume accounts for 3%-12%; water reducer 0.4%-1.3%; water-cement ratio 0.6-1.2; volume ratio 1:1-2.5:1).

3. The silica fume modified two-liquid grouting material according to claim 1, characterized in that: Liquid B includes the following components in parts by mass: 245 to 370 parts of water glass.

4. The silica fume modified two-liquid grouting material according to claim 3, characterized in that: Water glass is liquid sodium silicate water glass with a modulus of 3.03 to 3.3 and a Baume degree of 38.5 to 41.5°Bé.

5. The silica fume modified two-liquid grouting material according to claim 1, characterized in that: Silica fume has a silicon dioxide content of 98% and a particle size of 2.6 microns.

6. The silica fume modified two-liquid grouting material according to claim 1, characterized in that: The water reducer is a polycarboxylic acid high efficiency water reducer.

7. The silica fume modified two-liquid grouting material according to claim 1, characterized in that: Ordinary Portland cement, water, silica fume and water reducing agent are uniformly mixed, wherein the water-cement ratio is 0.6-1.2, and liquid A and liquid B are mixed at a volume ratio of 1:1-2.5:1 to obtain a silica fume modified two-liquid grouting material.

8. The silica fume modified two-liquid grouting material according to claim 1, characterized in that: Also disclosed is a method for preparing a silica fume modified double-liquid grouting material, comprising the following steps: Step 1: The factors that affect the basic properties of the two-liquid grouting material are: water-cement ratio, volume ratio, silica fume dosage, and water-reducing agent dosage; the experience level range of each factor is determined by relevant engineering experience and published results, and then the level of each factor in the orthogonal experimental scheme is determined; the orthogonal experimental scheme is to conduct an orthogonal combination design of the factors and the corresponding level numbers selected to determine the specific experimental scheme; Step 2: The basic properties of the two-liquid grouting material (setting time, water separation rate, stone rate and compressive strength) were tested by referring to the standards JGJT21110 "Technical Specifications for Cement-Water Glass Two-Liquid Grouting in Construction Engineering", DL / T5150-2001 "Testing Procedures for Hydraulic Concrete", and GB / T 50081 "Standard for Test Methods for Physical and Mechanical Properties of Concrete"; Step 3: The trend graph is a relationship graph between different levels of each factor and the evaluation index, including positive correlation and negative correlation trend graphs: the horizontal axis of the trend graph is the different levels of the research factors, and the vertical axis is the evaluation index. The extreme value of each factor level is used as the evaluation index of the degree of influence. The change rate of material performance is obtained after the basic characteristics test of the double-liquid grouting material is designed by the orthogonal experimental method. After processing the orthogonal experimental data results, the significant level of the influence of each factor on the basic performance of the slurry is found, and the optimal ratio is obtained as 12% silica fume, 0.8 water-cement ratio, 1.5:1 volume ratio, and 1.0% water reducer; Step 4: The water-cement ratio of the traditional single-liquid grouting material is the same as the water-cement ratio of the silica fume modified two-liquid grouting material with the optimal ratio obtained by orthogonal experiment; the water-cement ratio and volume ratio of the traditional two-liquid grouting material are also the same. The mechanical properties and durability of the silica fume modified two-liquid grouting material with the optimal ratio are compared with the traditional single-liquid grouting material and the traditional two-liquid grouting material, specifically the compressive strength comparison under different curing environments and ages, the water corrosion resistance and the impermeability comparison, with reference to GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete".

Citation Information

Patent Citations

  • Material and method for two-shot grouting used for soft soil roadbed reinforcement

    CN108585745A

Cited By

  • Double-liquid cement-based grouting material as well as preparation method and application thereof

    CN121405432A