P-N-S multi-element synergistic flame retardant and preparation method thereof
Through the two-step one-pot synthesis of P-N-S multi-element synergistic flame retardant, the problems of existing flame retardants affecting the light transmittance and mechanical properties of epoxy resins are solved, and efficient and environmentally friendly flame retardant performance and transparency are achieved. in microelectronics and optical materials.
Patent Information
- Application Number
- CN202411218537.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing phosphophenol structure reactive flame retardants will affect their light transmittance and mechanical properties when added to epoxy resins, and the color of conventional flame retardants will cause the product to be opaque.
The P-N-S multi-element synergistic flame retardant is synthesized by a two-step one-pot method of 2-amino-1,3,4-thiadiazole, thiophene formaldehyde and DOPO. The resulting white powder solid flame retardant has a simple molecular structure. It can be well compatible with epoxy resin, improving its flame retardant properties and transparency.
The flame retardant can achieve V-0 flame retardant performance at low addition amount, maintaining the mechanical properties and transparency of the epoxy resin, and also has the advantages of non-toxic and environmental protection. The synthesis process is simple and efficient, and the solvent is easy to recover.
Smart Images

Figure CN118994248A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of organic synthesis, and in particular to a PNS multi-element synergistic flame retardant and a preparation method thereof. Background Art
[0002] Epoxy resin is a highly applicable thermosetting resin with many excellent properties, such as high temperature resistance, solvent resistance, transparency, insulation, corrosion resistance, etc. It is widely used in microelectronics, paint coatings, construction, optics and other industries. However, epoxy resin is flammable and will also produce dripping and toxic smoke in the event of a fire. This limits its application in cutting-edge industries. The development of flame-retardant epoxy resins with excellent flame retardant properties is of great value to the promotion of its application.
[0003] 9,10-Dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) can be directly added to the resin, or it can be used as a flame retardant intermediate to synthesize a more efficient flame retardant. Its active PH bond can react with a variety of groups such as hydroxyl, carbonyl, amino, double bond, etc., and the product derivatization ability is very strong.
[0004] However, although the current flame retardants can improve the flame retardancy of resins, they often affect the light transmittance and mechanical properties of epoxy resins. For example, Chinese patent CN1065544483A discloses a phosphaphenanthrene structure reactive flame retardant and its application, wherein 5-aminomethyl-1,3-diphenyl-1,3,5-diazaphosphorus heterocyclic-substance I, 4-hydroxybenzaldehyde, DOPO and solvent are added as a catalyst, and the temperature is raised for a period of time to obtain a light yellow solution, which is concentrated, the solvent is removed, and the obtained substance is separated by column chromatography to obtain a phosphaphenanthrene structure reactive flame retardant. Although this method has -NH and can react with epoxy groups, it contains 12 benzene rings, which have great steric hindrance and are not easy to react with epoxy groups, which often causes part of the flame retardant to be insoluble before curing, resulting in the final resin product being opaque, and at the same time affecting the mechanical properties of the resin to a certain extent. Summary of the invention
[0005] The problem in the prior art is that the conventional phosphaphenanthrene structure reactive flame retardant itself has color, and when added to the epoxy resin material system, it will affect the light transmittance of the obtained epoxy resin flame retardant product. In view of the above problem, the present invention provides a PNS multi-element synergistic flame retardant, and its chemical structure is as follows:
[0006]
[0007] Preferably, the preparation method of the PNS multi-element synergistic flame retardant comprises the following steps:
[0008] 2-Amino-1,3,4-thiadiazole is added to an organic solvent, and then the temperature is raised to 60-80°C and stirred to dissolve completely. Thiophene carboxaldehyde is then added dropwise to the reaction system and the reaction is carried out at a constant temperature of 40-80°C for 6-12 hours. DOPO is then added to the reaction system and stirred evenly. The reaction is carried out at a constant temperature of 40-80°C for 12-24 hours. After the reaction is completed, the reaction liquid is filtered, washed with anhydrous ethanol, and vacuum dried to obtain a white powdery solid product, namely, PNS multi-element synergistic flame retardant.
[0009] Preferably, the organic solvent includes at least one of anhydrous ethanol, n-propanol, ethylene dichloride, tetrahydrofuran and acetonitrile.
[0010] Preferably, the usage ratio of 2-amino-1,3,4-thiadiazole to thiophenecarboxaldehyde and organic solvent is 0.02 mol:150 mL.
[0011] Preferably, the molar ratio of 2-amino-1,3,4-thiadiazole to thiophenecarboxaldehyde and DOPO is 1:1:1.
[0012] Preferably, the vacuum drying temperature is 80-100° C. and the drying time is 12-24 h.
[0013] A flame retardant epoxy resin, wherein the formula of the resin contains the PNS multi-element synergistic flame retardant obtained by the invention.
[0014] Preferably, the flame retardant epoxy resin comprises the following components in terms of weight percentage:
[0015] PNS multi-element synergistic flame retardant 0-10%;
[0016] Curing agent 15-20%;
[0017] Epoxy resin residue.
[0018] Preferably, the curing agent includes one or both of 4,4'-diaminodiphenyl sulfone and 4,4'-diaminodiphenylmethane.
[0019] The present invention has the following beneficial effects:
[0020] (1) The PNS multi-element synergistic flame retardant obtained by the present invention is synthesized by a two-step one-pot method using thiophene carboxaldehyde, 2-amino-1,3,4-thiadiazole and DOPO. The PNS multi-element synergistic flame retardant can effectively improve the flame retardancy of the epoxy resin material system, wherein the Schiff base intermediate MBTFA (generated by the reaction of thiophene carboxaldehyde and 2-amino-1,3,4-thiadiazole) has no benzene ring, has a simple molecular structure, has low steric hindrance, and has a higher reaction conversion rate;
[0021] (2) The PNS multi-element synergistic flame retardant obtained by the present invention has a simple and stable configuration, low structural rigidity, and is well compatible with epoxy resin. The flame retardant MBTFP can be evenly dispersed in the epoxy resin, and the flame retardant epoxy resin has stable flame retardant properties while also ensuring that the flame retardant epoxy resin has good mechanical properties and transparency. The flame retardant epoxy resin is expected to be used in microelectronic packaging and optical materials;
[0022] (3) The PNS multi-element synergistic flame retardant obtained by the present invention has good flame retardancy through molecular design. When the addition amount of the PNS multi-element synergistic flame retardant in the epoxy resin system is 2wt%, the flame retardancy of the epoxy resin product obtained can reach V-1 level (UL-94). When the addition amount of the PNS multi-element synergistic flame retardant in the epoxy resin system is 4wt%, the flame retardancy of the epoxy resin product obtained can reach V-0 level (UL-94). A lower addition amount can achieve higher flame retardancy, thereby reducing the influence of excessive addition of the PNS multi-element synergistic flame retardant on the mechanical properties of the epoxy resin;
[0023] (4) The PNS multi-element synergistic flame retardant obtained by the present invention is a reactive flame retardant, which can react with epoxy groups through -NH-, so that the flame retardant can be well dissolved in epoxy resin, thereby maintaining the transparency of epoxy resin; compared with halogen flame retardants, it has the advantages of being non-toxic, environmentally friendly, and safe; at the same time, the reaction adopts low temperature, normal pressure and two-step one-pot synthesis, the reaction is simple and efficient, the solvent and anhydrous ethanol in the reaction and purification stages are easy to recycle and reuse, and the economic benefits are considerable. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 : Infrared spectrum of the PNS multi-element synergistic flame retardant obtained in Example 1.
[0025] Figure 2 : H NMR spectrum of the PNS multi-element synergistic flame retardant obtained in Example 1.
[0026] Figure 3 : Nuclear magnetic resonance phosphorus spectrum analysis diagram of the PNS multi-element synergistic flame retardant obtained in Example 1.
[0027] Figure 4 : Transmittance test diagram of the flame retardant epoxy resin obtained in Example 1, in which MBTFP-2 represents flame retardant epoxy resin I, and MBTFP-4 represents flame retardant epoxy resin II.
[0028] Figure 5 : SEM image of the residual carbon of the flame retardant epoxy resin obtained in Example 1. In the figure, EP / MBTFP-2 represents flame retardant epoxy resin I, and EP / MBTFP-2 represents flame retardant epoxy resin II. DETAILED DESCRIPTION
[0029] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.
[0030] Example 1
[0031] A PNS multi-element synergistic flame retardant, the preparation method of which is as follows:
[0032] 0.02 mol 2-amino-1,3,4-thiadiazole was added to 150 mL of anhydrous ethanol, and then the temperature was raised to 80°C, and the mixture was stirred to dissolve completely. Then 0.02 mol thiophene carboxaldehyde was added dropwise to the reaction system, and the mixture was kept at a constant temperature of 80°C for 12 hours. Then 0.02 mol DOPO was added to the reaction system, and the mixture was stirred evenly, and the mixture was kept at a constant temperature of 80°C for 12 hours. After the reaction, the reaction liquid was filtered, washed with anhydrous ethanol, and vacuum dried at 80°C for 24 hours to obtain a white powdery solid product, namely, the PNS multi-element synergistic flame retardant. The filtration process was rinsed and filtered four times with 200 mL of anhydrous ethanol. The yield of the obtained PNS multi-element synergistic flame retardant was 78.5%, and its infrared spectrum is shown in the attached manual. Figure 1 As shown, the spectrum is: -NH-(3212cm -1 ); C=N(1633cm -1 ); P = O (1238cm -1 ); P-0-Ar(1204cm -1 , 921cm -1 ); PC(759cm -1 The NMR hydrogen spectrum of the obtained PNS multi-element synergistic flame retardant is shown in the attached manual. Figure 2 As shown, the hydrogen spectrum results are: 1 HNMR (DMSO-d6, 500MHz), δ (ppm): 7.00-8.32 (Ar-H); 6.63-6.99 (NH); 6.65-6.77 (C*-H).
[0033] The nuclear magnetic resonance phosphorus spectrum analysis diagram of the obtained PNS multi-element synergistic flame retardant is as shown in the attached manual. Figure 3 As shown, the results of the spectrum analysis are: 31 PNMR (DMS0-d6, 400MHz), (ppm): 39.44ppm (PC).
[0034] Flame retardant epoxy resin I, calculated by weight percentage, has the following composition:
[0035] PNS multi-element synergistic flame retardant 2%;
[0036] 4,4'-diaminodiphenylmethane 19.58%;
[0037] E51 margin.
[0038] Flame retardant epoxy resin II, calculated by weight percentage, has the following composition:
[0039] PNS multi-element synergistic flame retardant 4%;
[0040] 4,4'-diaminodiphenylmethane 18.98%;
[0041] E51 margin.
[0042] The preparation methods of flame retardant epoxy resin I and flame retardant epoxy resin II are carried out according to the following steps:
[0043] According to the formula, epoxy resin is weighed and heated to 160°C, PNS multi-element synergistic flame retardant is added to the molten system, stirred and dissolved, kept at a constant temperature for 8 minutes, slowly cooled to 90°C, added with the formula amount of curing agent, and the stirring speed is reduced. When the curing agent is completely dissolved, it is quickly added to the mold preheated at 100°C, cured at 100°C for 2 hours in a blast oven, and then cured at 150°C for 3 hours to obtain a flame retardant epoxy resin.
[0044] The flame retardant performance test data of flame retardant epoxy resin I, flame retardant epoxy resin II and pure epoxy resin are shown in Table 1.
[0045] Table 1
[0046]
[0047] Limiting oxygen index standard: ASTM D2863, specimen size: 130×6.5×3mm.
[0048] Vertical burning test standard: ASTM D3801, specimen size: 130×13×3mm.
[0049] The mechanical properties test data of flame retardant epoxy resin I, flame retardant epoxy resin II and pure epoxy resin are shown in Table 2.
[0050] Table 2
[0051]
[0052] Example 2
[0053] A PNS multi-element synergistic flame retardant, the preparation method of which is as follows:
[0054] 0.02 mol 2-amino-1,3,4-thiadiazole was added to 150 mL n-propanol, and then the temperature was raised to 80 ° C, and the mixture was stirred and dissolved completely. Then 0.02 mol thiophene carboxaldehyde was added dropwise to the reaction system, and the mixture was kept at 80 ° C for 12 hours. Then 0.02 mol DOPO was added to the reaction system, and the mixture was stirred evenly, and the mixture was kept at 80 ° C for 12 hours. After the reaction, the reaction liquid was filtered, washed with anhydrous ethanol, and vacuum dried at 80 ° C for 24 hours to obtain a white powder solid product, namely, PNS multi-element synergistic flame retardant. The filtration process was rinsed and filtered four times with 200 mL of anhydrous ethanol. The yield of the obtained PNS multi-element synergistic flame retardant was 73.9%.
[0055] Flame retardant epoxy resin III, calculated by weight percentage, has the following components:
[0056] PNS multi-element synergistic flame retardant 2%;
[0057] 4,4'-diaminodiphenylmethane 19.58%;
[0058] E51 margin.
[0059] Flame retardant epoxy resin IV, calculated by weight percentage, has the following components:
[0060] PNS multi-element synergistic flame retardant 4%;
[0061] 4,4'-diaminodiphenylmethane 18.98%;
[0062] E51 margin.
[0063] The preparation methods of flame retardant epoxy resin III and flame retardant epoxy resin IV are carried out according to the following steps:
[0064] According to the formula, epoxy resin is weighed and heated to 160°C, PNS multi-element synergistic flame retardant is added to the molten system, stirred and dissolved, kept at a constant temperature for 8 minutes, slowly cooled to 90°C, added with the formula amount of curing agent, and the stirring speed is reduced. When the curing agent is completely dissolved, it is quickly added to the mold preheated at 100°C, cured at 100°C for 2 hours in a blast oven, and then cured at 150°C for 3 hours to obtain a flame retardant epoxy resin.
[0065] The flame retardant performance test data of flame retardant epoxy resin III, flame retardant epoxy resin IV and pure epoxy resin are shown in Table 3.
[0066] Table 3
[0067]
[0068] Limiting oxygen index standard: ASTM D2863, specimen size: 130×6.5×3mm.
[0069] Vertical burning test standard: ASTM D3801, specimen size: 130×13×3mm.
[0070] The mechanical properties test data of flame retardant epoxy resin III, flame retardant epoxy resin IV and pure epoxy resin are shown in Table 4.
[0071] Table 4
[0072]
[0073] Example 3
[0074] A PNS multi-element synergistic flame retardant, the preparation method of which is as follows:
[0075] 0.02 mol of 2-amino-1,3,4-thiadiazole was added to 150 mL of dichloroethane, and then the temperature was raised to 80 ° C, and the mixture was stirred and dissolved completely. Then 0.02 mol of thiophene carboxaldehyde was added dropwise to the reaction system, and the mixture was kept at 80 ° C for 12 hours. Then 0.02 mol of DOPO was added to the reaction system, and the mixture was stirred evenly, and the mixture was kept at 80 ° C for 12 hours. After the reaction, the reaction solution was filtered, washed with anhydrous ethanol, and vacuum dried at 80 ° C for 24 hours to obtain a white powder solid product, namely, PNS multi-element synergistic flame retardant. The filtration process was rinsed and filtered four times with 200 mL of anhydrous ethanol. The yield of the obtained PNS multi-element synergistic flame retardant was 76.3%.
[0076] Flame retardant epoxy resin III, calculated by weight percentage, has the following components:
[0077] PNS multi-element synergistic flame retardant 2%;
[0078] 4,4'-diaminodiphenylmethane 19.58%;
[0079] E51 margin.
[0080] Flame retardant epoxy resin IV, calculated by weight percentage, has the following components:
[0081] PNS multi-element synergistic flame retardant 4%;
[0082] 4,4'-diaminodiphenylmethane 18.98%;
[0083] E51 margin.
[0084] The preparation methods of flame retardant epoxy resin V and flame retardant epoxy resin VI are carried out according to the following steps:
[0085] According to the formula, epoxy resin is weighed and heated to 160°C, PNS multi-element synergistic flame retardant is added to the molten system, stirred and dissolved, kept at a constant temperature for 8 minutes, slowly cooled to 90°C, added with the formula amount of curing agent, and the stirring speed is reduced. When the curing agent is completely dissolved, it is quickly added to the mold preheated at 100°C, cured at 100°C for 2 hours in a blast oven, and then cured at 150°C for 3 hours to obtain a flame retardant epoxy resin.
[0086] The flame retardant performance test data of flame retardant epoxy resin V, flame retardant epoxy resin VI and pure epoxy resin are shown in Table 5.
[0087] Table 5
[0088]
[0089] Limiting oxygen index standard: ASTM D2863, specimen size: 130×6.5×3mm.
[0090] Vertical burning test standard: ASTM D3801, specimen size: 130×13×3mm.
[0091] The mechanical properties test data of flame retardant epoxy resin III, flame retardant epoxy resin IV and pure epoxy resin are shown in Table 6.
[0092] Table 6
[0093]
[0094] Example 4
[0095] A PNS multi-element synergistic flame retardant, the preparation method of which is as follows:
[0096] 0.02 mol of 2-amino-1,3,4-thiadiazole was added to 150 mL of tetrahydrofuran, and then the temperature was raised to 80 ° C, and the mixture was stirred and dissolved completely. Then 0.02 mol of thiophene carboxaldehyde was added dropwise to the reaction system, and the mixture was kept at 80 ° C for 12 hours. Then 0.02 mol of DOPO was added to the reaction system, and the mixture was stirred evenly, and the mixture was kept at 80 ° C for 12 hours. After the reaction, the reaction liquid was filtered, washed with anhydrous ethanol, and vacuum dried at 80 ° C for 24 hours to obtain a white powder solid product, namely, PNS multi-element synergistic flame retardant. The filtration process was rinsed and filtered four times with 200 mL of anhydrous ethanol. The yield of the obtained PNS multi-element synergistic flame retardant was 72.5%.
[0097] Flame retardant epoxy resin VII, calculated by weight percentage, has the following composition:
[0098] PNS multi-element synergistic flame retardant 2%;
[0099] 4,4'-diaminodiphenylmethane 19.58%;
[0100] E51 margin.
[0101] Flame retardant epoxy resin VIII, calculated by weight percentage, has the following composition:
[0102] PNS multi-element synergistic flame retardant 4%;
[0103] 4,4'-diaminodiphenylmethane 18.98%;
[0104] E51 margin.
[0105] The preparation methods of flame retardant epoxy resin VII and flame retardant epoxy resin VIII are carried out according to the following steps:
[0106] According to the formula, epoxy resin is weighed and heated to 160°C, PNS multi-element synergistic flame retardant is added to the molten system, stirred and dissolved, kept at a constant temperature for 8 minutes, slowly cooled to 90°C, added with the formula amount of curing agent, and the stirring speed is reduced. When the curing agent is completely dissolved, it is quickly added to the mold preheated at 100°C, cured at 100°C for 2 hours in a blast oven, and then cured at 150°C for 3 hours to obtain a flame retardant epoxy resin.
[0107] The flame retardant performance test data of flame retardant epoxy resin VII, flame retardant epoxy resin VIII and pure epoxy resin are shown in Table 7.
[0108] Table 7
[0109]
[0110] Limiting oxygen index standard: ASTM D2863, specimen size: 130×6.5×3mm.
[0111] Vertical burning test standard: ASTM D3801, specimen size: 130×13×3mm.
[0112] The mechanical property test data of flame retardant epoxy resin III, flame retardant epoxy resin IV and pure epoxy resin are shown in Table 8.
[0113] Table 8
[0114]
[0115] Example 5
[0116] A PNS multi-element synergistic flame retardant, the preparation method of which is as follows:
[0117] 0.02 mol 2-amino-1,3,4-thiadiazole was added to 150 mL acetonitrile, and then the temperature was raised to 80 ° C, and the mixture was stirred and dissolved completely. Then 0.02 mol thiophene carboxaldehyde was added dropwise to the reaction system, and the mixture was kept at 80 ° C for 12 hours. Then 0.02 mol DOPO was added to the reaction system, and the mixture was stirred evenly, and the mixture was kept at 80 ° C for 12 hours. After the reaction, the reaction solution was filtered, washed with anhydrous ethanol, and vacuum dried at 80 ° C for 24 hours to obtain a white powder solid product, namely, PNS multi-element synergistic flame retardant. The filtration process was rinsed and filtered four times with 200 mL of anhydrous ethanol. The yield of the obtained PNS multi-element synergistic flame retardant was 72.5%.
[0118] Flame retardant epoxy resin IX, calculated by weight percentage, has the following composition:
[0119] PNS multi-element synergistic flame retardant 2%;
[0120] 4,4'-diaminodiphenylmethane 19.58%;
[0121] E51 margin.
[0122] Flame retardant epoxy resin X, calculated by weight percentage, has the following composition:
[0123] PNS multi-element synergistic flame retardant 4%;
[0124] 4,4'-diaminodiphenylmethane 18.98%;
[0125] E51 margin.
[0126] The preparation methods of flame retardant epoxy resin IX and flame retardant epoxy resin X are carried out according to the following steps:
[0127] According to the formula, epoxy resin is weighed and heated to 160°C, PNS multi-element synergistic flame retardant is added to the molten system, stirred and dissolved, kept at a constant temperature for 8 minutes, slowly cooled to 90°C, added with the formula amount of curing agent, and the stirring speed is reduced. When the curing agent is completely dissolved, it is quickly added to the mold preheated at 100°C, cured at 100°C for 2 hours in a blast oven, and then cured at 150°C for 3 hours to obtain a flame retardant epoxy resin.
[0128] The flame retardant performance test data of flame retardant epoxy resin IX, flame retardant epoxy resin X, and pure epoxy resin are shown in Table 9.
[0129] Table 9
[0130]
[0131] Limiting oxygen index standard: ASTM D2863, specimen size: 130×6.5×3mm.
[0132] Vertical burning test standard: ASTM D3801, specimen size: 130×13×3mm.
[0133] The mechanical property test data of flame retardant epoxy resin IX, flame retardant epoxy resin X and pure epoxy resin are shown in Table 10.
[0134] Table 10
[0135]
[0136] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A PNS multi-element synergistic flame retardant, characterized in that: The chemical structure is as follows:
2. A PNS multi-element synergistic flame retardant according to claim 1, characterized in that: The preparation method comprises the following steps: 2-Amino-1,3,4-thiadiazole is added to an organic solvent, and then the temperature is raised to 60-80°C and stirred to dissolve completely. Thiophene carboxaldehyde is then added dropwise to the reaction system and the reaction is carried out at a constant temperature of 40-80°C for 6-12 hours. DOPO is then added to the reaction system and stirred evenly. The reaction is carried out at a constant temperature of 40-80°C for 12-24 hours. After the reaction is completed, the reaction liquid is filtered, washed with anhydrous ethanol, and vacuum dried to obtain a white powdery solid product, namely, PNS multi-element synergistic flame retardant.
3. A PNS multi-element synergistic flame retardant according to claim 2, characterized in that: The organic solvent includes at least one of anhydrous ethanol, n-propanol, ethylene dichloride, tetrahydrofuran and acetonitrile.
4. A PNS multi-element synergistic flame retardant according to claim 2, characterized in that: The usage ratio of 2-amino-1,3,4-thiadiazole to thiophenecarboxaldehyde and organic solvent is 0.02 mol:150 mL.
5. A PNS multi-element synergistic flame retardant according to claim 2, characterized in that: The molar ratio of 2-amino-1,3,4-thiadiazole to thiophenecarboxaldehyde and DOPO is 1:1:
1.
6. A PNS multi-element synergistic flame retardant according to claim 1, characterized in that: The vacuum drying temperature is 80-100°C and the drying time is 12-24h.
7. A flame retardant epoxy resin, characterized in that: The formula contains the PNS multi-element synergistic flame retardant obtained according to any one of claims 1 to 6.
8. A flame retardant epoxy resin according to claim 7, characterized in that: The composition is calculated by weight percentage and includes the following ingredients: PNS multi-element synergistic flame retardant 0-10%; Curing agent 15-20%; Epoxy resin residue.
9. A flame retardant epoxy resin according to claim 8, characterized in that: The curing agent includes one or two of 4,4'-diaminodiphenyl sulfone and 4,4'-diaminodiphenylmethane.
Citation Information
Cited By
Nitrogen-rich DOPO-based flame retardant and synthesis and application thereof
CN120118124A
Diphenylphosphine oxide derivative flame retardant for thermoplastic resin as well as preparation method and application of diphenyl phosphine oxide derivative flame retardant
CN122483107A
Flame retardant for thermoplastic resins, process for its preparation and use
CN122483107B