Bismuth metal organic framework hollow material as well as preparation method and application thereof
Bi-MOF, a bismuth metal organic frame hollow material prepared by solvent thermal reaction, is used for the negative electrode of lithium-ion batteries, solving the problem of low anode capacity in lithium-ion batteries, achieving high cycling stability and rate performance of the material, and complying with environmental protection and economical production requirements.
Patent Information
- Application Number
- CN202411097034.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-22
AI Technical Summary
The theoretical capacity of graphite as the anode material in existing lithium-ion batteries is low, which leads to volume expansion of lithium-ion batteries during circulation, resulting in reduced electrode integrity, thereby reducing ion conductivity and Li+ migration rate, limiting the further development of lithium-ion batteries. .
Bi-MOF is prepared by solvent-thermal reaction, and the bismuth metal organic frame hollow material Bi-MOF is used to carry out magnetic stirring reaction in alcohol and amide solvents using bismuth salt and organic acid ligand to form Bi-MOF material with hollow structure and is used for lithium ion Battery negative electrode material.
Bi-MOF materials show excellent electrochemical properties, have good porosity and high ionic conductivity, which significantly improves the cycle stability and rate performance of lithium-ion batteries. They also have rich raw materials, low cost, simple preparation process, and meet the environment. Friendship principle.
Smart Images

Figure CN118994616A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal organic framework materials, and in particular relates to a bismuth metal organic framework hollow material and a preparation method and application thereof. Background Art
[0002] With the development of new energy technology, the development and design of economical, green and environmentally friendly renewable energy storage technology has entered the public's field of vision and become a hot topic. Lithium-ion batteries have been widely used in electronics, aerospace and other industries due to their green and environmentally friendly, high capacity and long cycle life. However, lithium-ion batteries with graphite as anode material face the problem of low theoretical capacity (372mAh g -1 ) and other issues restrict its further development.
[0003] Bismuth (Bi) is a promising anode material with the characteristics of high natural abundance, low cost, green and non-toxic, and environmentally friendly. It also has a unique layered crystal structure with an interlayer spacing of It provides enough space for the insertion and extraction of lithium ions during the cycle. Like other negative electrode materials, Bi will also undergo a dramatic volume expansion during the cycle, destroying the integrity of the electrode and slowing down the Li + The migration rate of Bi decreases and the ionic conductivity decreases, which leads to capacity decay when Bi is used as the negative electrode of lithium-ion batteries. In order to overcome the above obstacles and promote the rapid occurrence of electrochemical reactions, the construction and design of porous materials with high specific surface area has attracted great attention. Among them, metal organic frameworks with highly controllable structure, adjustable porosity, large specific surface area, and easy functionalization are the preferred carrier materials for electrode materials.
[0004] The prior art discloses a method for a ladder-type Bi-MOF-M / CdS / Bi2S3 heterojunction visible light catalyst, which uses bismuth salt and 2-aminoterephthalic acid to coordinate under a solvent thermal reaction to obtain amino-functionalized Bi-MOF microspheres, which are used in the catalytic field.
[0005] The prior art also discloses a bismuth-based metal organic framework nanomaterial with a central metal Bi 3+ As the connecting node, the organic ligand is used as a bridge to connect with Bi 3+ Planar or three-dimensional network structured porous nanomaterials are formed by chelation coordination and are used in photoacoustic diagnosis of tumors.
[0006] So far, there is no relevant literature reporting the preparation method of bismuth metal organic framework hollow materials and their application in battery negative electrodes. Summary of the invention
[0007] The purpose of the present invention is to provide a bismuth metal organic framework hollow material and its preparation method and application. The present invention obtains a bismuth metal organic framework material Bi-MOF by a solvothermal reaction. Compared with the prior art, the significant advantages of the present invention are that the raw materials used are not only widely available and low in cost, but also the equipment required in the preparation process is simple, and the entire production process complies with environmentally friendly principles. In addition, the present invention has a high degree of repeatability, ensuring the consistency and stability of material production. More importantly, the hollow structure design of Bi-MOF gives it excellent electrochemical performance in the field of batteries, indicating broad application potential.
[0008] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is:
[0009] A method for preparing a bismuth metal organic framework hollow material comprises the following steps:
[0010] (1) dissolving a bismuth salt in an alcohol solvent to obtain a bismuth salt solution; dissolving an organic acid ligand in an amide solvent to obtain an organic acid ligand solution;
[0011] (2) mixing the organic acid ligand solution and the bismuth salt solution uniformly under magnetic stirring, and subjecting the obtained mixed solution to a solvothermal reaction;
[0012] (3) After the solvothermal reaction in step (2) is completed, the mixture is cooled to room temperature and post-treated to obtain a powdery product, which is labeled as Bi-MOF.
[0013] Furthermore, in step (1), the bismuth salt is a mixture of one or more of bismuth chloride, bismuth nitrate, bismuth carbonate, and bismuth acetate; and the organic acid ligand is a mixture of one or more of 1,3,5-benzenetricarboxylic acid, terephthalic acid, 2-aminoterephthalic acid, and 4,4'-biphenyldicarboxylic acid.
[0014] Furthermore, in step (1), the alcohol solvent is a mixture of one or more of ethanol, methanol, and ethylene glycol; the amide solvent is a mixture of one or two of N,N-dimethylformamide and N,N-dimethylacetamide.
[0015] Furthermore, in step (1), the molar ratio of the bismuth salt to the organic acid ligand is 1:10-10:1, preferably 1:4-1:1.
[0016] Furthermore, in step (1), the concentration of the bismuth salt is 0.025-0.25 mmol / mL, preferably 0.025-0.05 mmol / mL; the concentration of the organic acid ligand is 0.03-0.3 mmol / mL, preferably 0.06-0.13 mmol / mL.
[0017] Furthermore, in step (2), the temperature of the solvent thermal reaction is 80-180° C., preferably 150° C., and the reaction time is 3-96 h, preferably 16 h.
[0018] Furthermore, in step (3), the post-treatment includes solid-liquid separation, washing and drying of the reaction product.
[0019] Furthermore, in step (3), the post-treatment is to centrifuge or filter the reaction product to obtain a precipitate, and then wash the precipitate with a mixture of one or more of ethanol, N,N-dimethylformamide, formamide, methanol, ethylene glycol or deionized water, and the washed precipitate is vacuum dried at 40-90°C.
[0020] The invention provides a bismuth metal organic framework hollow material prepared by the above preparation method.
[0021] The present invention also provides application of the above-mentioned bismuth metal organic framework hollow material in battery negative electrode materials.
[0022] Compared with the prior art, the present invention has the following advantages:
[0023] (1) The bismuth metal organic framework Bi-MOF provided by the present invention is a hollow material with good crystallization and uniform particle size distribution, and has the advantages of good porosity and high ionic conductivity.
[0024] (2) Compared with existing materials, the bismuth metal organic framework Bi-MOF hollow material provided by the present invention has the advantages of abundant and low-cost raw materials, simple equipment required, and environmental friendliness. It has high experimental repeatability and a unique hollow structure that exhibits excellent electrochemical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 XRD pattern of Bi-MOF obtained in Example 1;
[0026] Figure 2 This is the SEM image of the Bi-MOF obtained in Example 1;
[0027] Figure 3 The cycle performance diagram of Bi-MOF obtained in Example 1 and Bi NPs obtained in Comparative Example 1 in lithium-ion battery negative electrode materials;
[0028] Figure 4 This is a rate performance diagram of the Bi-MOF obtained in Example 1 and the Bi NPs obtained in Comparative Example 1 in lithium-ion battery negative electrode materials. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Example 1
[0031] A method for preparing a bismuth metal organic framework hollow material comprises the following steps:
[0032] (1) Weighing 2 mmol of bismuth nitrate and dissolving it in 40 mL of ethylene glycol to obtain a bismuth salt solution; weighing 3 mmol of terephthalic acid and dissolving it in 30 mL of N,N-dimethylformamide to obtain an organic acid ligand solution;
[0033] (2) Under magnetic stirring, the organic acid ligand solution and the bismuth salt solution are mixed evenly, and the resulting mixed solution is transferred into a polytetrafluoroethylene liner and loaded into the shell of a reactor for solvothermal reaction at a reaction temperature of 150° C. and a reaction time of 16 h;
[0034] (3) After the reaction was completed, the mixture was naturally cooled to room temperature, the product was collected and washed several times with deionized water and anhydrous ethanol, and dried in a drying oven at 60°C for 12 h to obtain a powdery product, which was labeled as Bi-MOF. The XRD pattern of the Bi-MOF material is shown in FIG. Figure 1 As shown in the SEM images Figure 2 shown.
[0035] Example 2
[0036] A method for preparing a bismuth metal organic framework hollow material comprises the following steps:
[0037] (1) Weighing 2 mmol of bismuth nitrate and dissolving it in 40 mL of ethylene glycol to obtain a bismuth salt solution; weighing 2 mmol of 2-aminoterephthalic acid and dissolving it in 30 mL of N,N-dimethylformamide to obtain an organic acid ligand solution;
[0038] (2) Under magnetic stirring, the organic acid ligand solution and the bismuth salt solution are mixed evenly, and the resulting mixed solution is transferred into a polytetrafluoroethylene liner and loaded into the shell of a reactor for solvothermal reaction at a reaction temperature of 150° C. and a reaction time of 16 h;
[0039] (3) After the reaction, the mixture was naturally cooled to room temperature, the product was collected and washed several times with deionized water and anhydrous ethanol, and dried in a drying oven at 60 °C for 12 h to obtain a powdered product, which was labeled as Bi-MOF.
[0040] Example 3
[0041] A method for preparing a bismuth metal organic framework hollow material comprises the following steps:
[0042] (1) Weighing 1 mmol of bismuth chloride and dissolving it in 40 mL of ethanol to obtain a bismuth salt solution; weighing 4 mmol of 4,4'-biphenyldicarboxylic acid and dissolving it in 30 mL of N,N-dimethylformamide to obtain an organic acid ligand solution;
[0043] (2) Under magnetic stirring, the organic acid ligand solution and the bismuth salt solution are mixed evenly, and the resulting mixed solution is transferred into a polytetrafluoroethylene liner and loaded into the shell of a reactor for solvothermal reaction at a reaction temperature of 150° C. and a reaction time of 16 h;
[0044] (3) After the reaction, the mixture was naturally cooled to room temperature, the product was collected and washed several times with deionized water and anhydrous ethanol, and dried in a drying oven at 60 °C for 12 h to obtain a powdered product, which was labeled as Bi-MOF.
[0045] Comparative Example 1:
[0046] (1) Weigh 2 mmol of bismuth nitrate and dissolve it in 40 mL of ethylene glycol to obtain a bismuth salt solution;
[0047] (2) Under magnetic stirring, the obtained bismuth salt solution and 30 mL of 1 M nitric acid were mixed evenly, and the obtained mixed solution was transferred into a polytetrafluoroethylene liner and loaded into the shell of a reactor for solvothermal reaction at a reaction temperature of 150° C. and a reaction time of 16 h;
[0048] (3) After the reaction, the mixture was naturally cooled to room temperature, the product was collected and washed several times with deionized water and anhydrous ethanol, and dried in a drying oven at 60 °C for 12 h to obtain a powdery product, which was labeled as Bi NPs.
[0049] Example 1 and Comparative Example 1 were used as negative electrode active materials for lithium-ion batteries, PVDF was used as a binder, SP was used as a conductive agent, and NMP was used as a solvent. The mixture was uniformly coated on copper foil at a mass ratio of m(active material): m(SuperP): m(PVDF) = 7:2:1, and then transferred to a vacuum drying oven at 80°C for drying for 12 hours. After drying, the electrode sheet was placed on a roller press and rolled, and cut into circular electrode sheets with a uniform thickness of 12 mm using a slicer. The mass was weighed and recorded, and the mass of the active material was calculated. The electrode sheet was placed in a constant temperature oven at 80°C for drying for 2 hours.
[0050] The CR-2025 button cell was assembled in a glove box filled with argon. The water pressure and oxygen pressure in the glove box were always kept below 0.01 ppm. The electrolyte was 1 mol·L -1 of LiPF6.
[0051] The materials in Example 1 and Comparative Example 1 were subjected to electrochemical performance tests and electrochemical specific capacity curves were obtained. The results are shown in FIG. Figure 3 and Figure 4 As shown. Figure 3 It can be seen that after 300 cycles, the specific capacity of Example 1 is 313.3 mAhg -1 , Comparative Example 1 is 115.1 mAhg -1 , indicating that the material of Example 1 has excellent cycle stability. Figure 4 It can be seen that at different current densities (0.1-10Ag -1 ), the discharge specific capacity of Example 1 is completely higher than that of Comparative Example 1, and has excellent rate performance.
[0052] The above description is a detailed description of the preferred feasible embodiments of the present invention, but the embodiments are not intended to limit the scope of the patent application of the present invention. All equivalent changes or modified changes completed under the technical spirit suggested by the present invention should fall within the patent scope covered by the present invention.
Claims
1. A method for preparing a bismuth metal organic framework hollow material, characterized in that: The following steps are involved: (1) dissolving a bismuth salt in an alcohol solvent to obtain a bismuth salt solution; dissolving an organic acid ligand in an amide solvent to obtain an organic acid ligand solution; (2) mixing the organic acid ligand solution and the bismuth salt solution uniformly under magnetic stirring, and subjecting the obtained mixed solution to a solvothermal reaction; (3) After the solvothermal reaction in step (2) is completed, the mixture is cooled to room temperature and post-treated to obtain a powdery product, which is labeled as Bi-MOF.
2. The method for preparing the bismuth metal organic framework hollow material according to claim 1, characterized in that: In step (1), the bismuth salt is a mixture of one or more of bismuth chloride, bismuth nitrate, bismuth carbonate, and bismuth acetate; the organic acid ligand is a mixture of one or more of 1,3,5-benzenetricarboxylic acid, terephthalic acid, 2-aminoterephthalic acid, and 4,4'-biphenyldicarboxylic acid.
3. The method for preparing the bismuth metal organic framework hollow material according to claim 1, characterized in that: In step (1), the alcohol solvent is a mixture of one or more of ethanol, methanol, and ethylene glycol; the amide solvent is a mixture of one or two of N,N-dimethylformamide and N,N-dimethylacetamide.
4. The method for preparing the bismuth metal organic framework hollow material according to claim 1, characterized in that: In step (1), the molar ratio of the bismuth salt to the organic acid ligand is 1:10-10:
1.
5. The method for preparing the bismuth metal organic framework hollow material according to claim 1, characterized in that: In step (1), the concentration of the bismuth salt is 0.025-0.25 mmol / mL; the concentration of the organic acid ligand is 0.03-0.3 mmol / mL.
6. The method for preparing the bismuth metal organic framework hollow material according to claim 1, characterized in that: In step (2), the temperature of the solvent thermal reaction is 80-180° C., and the reaction time is 3-96 hours.
7. The method for preparing the bismuth metal organic framework hollow material according to claim 1, characterized in that: In step (3), the post-treatment includes solid-liquid separation, washing and drying of the reaction product.
8. The method for preparing the bismuth metal organic framework hollow material according to claim 7, characterized in that: In step (3), the post-treatment is to centrifuge or filter the reaction product to obtain a precipitate, then wash the precipitate with a mixture of one or more of ethanol, N,N-dimethylformamide, formamide, methanol, ethylene glycol or deionized water, and the washed precipitate is vacuum dried at 40-90°C.
9. The bismuth metal organic framework hollow material obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the bismuth metal organic framework hollow material according to claim 9 in battery negative electrode materials.
Citation Information
Cited By
Preparation method and application of amorphous hollow tube spherical bismuth tungstate material
CN121044628A