Water-based intermediate coat for 3C1B1PH coating as well as preparation method and application of water-based intermediate coat
By adjusting the ratio of silicate compounds, thickeners and alcohol ether solvents in water-based medium coating, an aqueous medium coating with excellent sag resistance was developed, which solved the adverse problems caused by the extended leveling time in the coating assembly line. , which improves the appearance and performance of the paint film and reduces the cost of equipment transformation.
Patent Information
- Application Number
- CN202310555615.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-22
AI Technical Summary
When the existing automotive coating assembly line is transformed into a 3C1B1PH process, the middle coating leveling time is extended, resulting in poor problems such as sagging, mixing and surface dry inner layers, affecting the appearance and performance of the paint film.
Develop an aqueous medium-based paint with excellent anti-sag performance, containing polyurethane resin emulsion, aqueous acrylic emulsion, amino resin, RD dispersion, additives and alcohol ether solvents, by adjusting silicate compounds, thickeners and alcohols The ratio of ether solvents improves viscosity and surface drying speed, and is suitable for leveling time of more than 15 minutes.
The water-based paint has good anti-sag performance and fluidity under long-term leveling conditions, ensuring excellent appearance and good mechanical properties of the paint film. It is suitable for the extended leveling time caused by assembly line transformation, reducing the equipment The transformation cost and the normal operation of the coating assembly line is maintained.
Smart Images

Figure BDA0004232882560000091 
Figure BDA0004232882560000101 
Figure BDA0004232882560000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of coatings, and more specifically to a water-based mid-coat for 3C1B1PH coating, and a preparation method and application thereof. Background Art
[0002] With the increasing environmental protection requirements and customers' demand for cost reduction, the automotive coating industry has completed many reforms and developed a variety of mature automotive coating systems. Taking environmental factors into consideration and cooperating with the development of water-based coating technology, the current water-based coating system can be roughly divided into water-based 3C1B coating and water-based 3C2B coating. Compared with water-based 3C2B coating, water-based 3C1B coating omits the drying and polishing steps of the middle coating, which can significantly reduce the coating cost and operating cost. Therefore, it has become a mainstream trend of development at this stage, and then derived and developed a more compact and environmentally friendly 3C1B1PH "wet-on-wet" coating process.
[0003] However, due to the high cost of painting line transformation, in order to ensure that the old 3C2B line is not eliminated and can continue to operate normally, the existing OEM factories hope to implement the 3C1B1PH painting process based on the existing 3C2B old line to reduce the cost of equipment transformation. For this reason, OEM factories often directly shut down the midcoat pre-baking and baking equipment to implement the 3C1B1PH process. In this way, during the original midcoat pre-baking and baking process, the cars on the assembly line are actually still in the leveling process, which will cause the midcoat leveling time to be too long, increasing the risk of adverse problems such as sagging, mixed layers, and dry surface and wet inner layer, which will not only affect the subsequent spraying of color paint and clear coat, but also affect the final appearance of the paint film.
[0004] Therefore, based on the problem of prolonged leveling time caused by the transformation of the old 3C2B line process, it is very necessary to develop a water-based mid-coat with anti-sagging performance and long leveling time. Summary of the invention
[0005] To solve the above problems, the first object of the present invention is to provide a water-based mid-coat for 3C1B1PH coating. The water-based mid-coat of the present invention has good anti-sagging performance and suitable viscosity, is suitable for the situation of long leveling time (more than 15 minutes), and the final paint film has excellent appearance, good mechanical properties and chemical properties.
[0006] A second object of the present invention is to provide a method for preparing the water-based mid-coat paint as described above.
[0007] The third object of the present invention is to provide an application of the water-based mid-coat paint as described above in the automotive 3C1B1PH coating process.
[0008] To achieve the above first object, the technical solution of the present invention is as follows:
[0009] The present invention discloses a water-based mid-coat for 3C1B1PH coating, comprising the following components in parts by weight:
[0010] 24-32 parts of polyurethane resin emulsion;
[0011] 2-4 parts of polyurethane resin;
[0012] 4-8 parts of water-based acrylic emulsion;
[0013] 5-7 parts of amino resin;
[0014] RD dispersion 4-10 parts;
[0015] 2.5-6.5 parts of additives;
[0016] 2.5-8 parts of alcohol ether solvent;
[0017] 20-30 parts water;
[0018] Wherein, the auxiliary agent comprises a thickener and a modified polyol; the RD dispersion comprises a silicate compound;
[0019] The mass ratio of the silicate compound, the thickener and the alcohol ether solvent is 0.12-0.3:1-2:2.5-8.
[0020] Furthermore, the mass ratio of the silicate compound, the thickener, the alcohol ether solvent and the modified polyol is 0.12-0.3:1-2:2.5-8:0.2-0.5.
[0021] Furthermore, the mass ratio of the silicate compound, the thickener, the alcohol ether solvent and the modified polyol is 0.165:1.5:3:0.2.
[0022] Furthermore, the thickener is selected from one or more of polyacrylate thickeners, polyurethane thickeners and polyamide wax thickeners;
[0023] The modified polyol is isotridecanol.
[0024] Further, the alcohol ether solvent comprises alcohol ether solvent A and alcohol ether solvent B;
[0025] Among them, the alcohol ether solvent A is diethylene glycol butyl ether, and the alcohol ether solvent B is selected from one or more of ethylene glycol butyl ether, isooctyl alcohol, isopropanol, ethylene glycol hexyl ether and ethylene glycol isooctyl ether.
[0026] Furthermore, the mass ratio of the silicate compound, the thickener, the alcohol ether solvent A, the alcohol ether solvent B and the modified polyol is 0.12-0.3:1-2:0.5-2:2-6:0.2-0.5.
[0027] Furthermore, the mass ratio of the silicate compound, the thickener, the alcohol ether solvent A, the alcohol ether solvent B and the modified polyol is 0.165:1.5:1:3:0.3.
[0028] Furthermore, the polyurethane resin emulsion comprises a wear-resistant polyurethane resin emulsion and / or a plasticized polyurethane emulsion.
[0029] Furthermore, the polyurethane resin emulsion comprises 20-24 parts by weight of wear-resistant polyurethane resin emulsion and 4-8 parts by weight of plasticizing polyurethane emulsion.
[0030] Furthermore, the wear-resistant polyurethane resin emulsion is selected from one or more of ETERANE VK5516, ETERANEVK563 and ETERANE VK505 of Changxing Company.
[0031] Furthermore, the plasticized polyurethane emulsion is selected from one or more of DAOTAN TW 6466 / 36WA, DAOTANTW 6431 / 45WA and DAOTAN VTW 6462 / 36WA of Allnex.
[0032] Furthermore, the amino resin comprises methyl etherified amino resin and / or imino amino resin.
[0033] Furthermore, the amino resin comprises 1-2 parts by weight of methyl etherified amino resin and 3-5 parts by weight of imino amino resin.
[0034] Furthermore, the methyl etherified amino resin is selected from one or more of CYMEL 303, CYMEL 308 and CYMEL 350 of Allnex.
[0035] Furthermore, the iminoamino resin is selected from one or more of CYMEL 325, CYMEL 327 and CYMEL 323 of Allnex.
[0036] Further, the RD dispersion is prepared by the following steps:
[0037] Under stirring conditions, 3 parts by weight of a silicate compound are slowly added to 60 parts by weight of water, followed by adding a total of 32 parts by weight of water in several times, stirring for 1-3 hours and then standing for at least 8 hours, then slowly adding 1.5 parts by weight of a polyether polyol and 3.5 parts by weight of water, stirring for 15-30 minutes, and standing for at least 8 hours again.
[0038] Furthermore, the silicate compound is selected from at least one of Laponite RD of BYK, Hatorite RD of Hemmings and Optigel CG of BYK; the silicate compound accounts for 0.12%-0.3% of the total weight of the water-based mid-coat.
[0039] Furthermore, the polyether polyol is selected from one or more of PX-1000, PPG 1000, PPG 2000 and GP-1000 of Sanyo Chemical.
[0040] Furthermore, the water-based mid-coat paint further comprises 20-25 parts by weight of titanium dioxide and 0-0.5 parts by weight of other pigments and fillers;
[0041] The other pigments and fillers are selected from one or more of carbon black, iron red, iron yellow, barium sulfate and talc.
[0042] To achieve the above second purpose, the technical solution of the present invention is as follows:
[0043] The present invention discloses a method for preparing the water-based mid-coat paint as described above, comprising the following steps:
[0044] Under stirring conditions, a portion of the polyurethane resin emulsion, a portion of the alcohol ether solvent, a portion of the auxiliary agent, and a portion of water are mixed, the pH of the system is adjusted to 8.1-8.3, the premix viscosity is controlled to be 100-120 KU, and then the obtained mixture is sand-milled to obtain a sand-milled slurry;
[0045] Add the remaining polyurethane resin emulsion, polyurethane resin, water-based acrylic emulsion, amino resin, RD dispersion, the remaining alcohol ether solvent, and the remaining additives to the sand-polished slurry, mix well, adjust the system pH to 8.2-8.6, and then add water to adjust the viscosity to 180-200 mPa.s to obtain the water-based mid-coat paint.
[0046] To achieve the third object, the technical solution of the present invention is as follows:
[0047] The present invention discloses an application of the water-based intermediate coating as described above in a 3C1B1PH coating process for automobiles, wherein the 3C1B1PH coating process comprises the following steps:
[0048] Sample electrophoresis treatment → spraying of mid-coat → mid-coat leveling → spraying of color paint → color paint leveling → color paint pre-baking → spraying of clear varnish → clear varnish leveling → clear varnish baking.
[0049] Furthermore, the paint film thickness of the intermediate paint is 12-14 μm.
[0050] Furthermore, the leveling time of the intermediate coating is 15-20 minutes.
[0051] The beneficial effects of the present invention are as follows:
[0052] The present invention discloses a water-based mid-coat for 3C1B1PH coating, which has the following advantages over the coating composition disclosed in the prior art:
[0053] 1. The present invention improves the storage stability and workability of the coating by adjusting the compounding relationship of the silicate compound, the thickener and the alcohol ether solvent in the formula on the basis of the traditional film-forming resin formula, so as to avoid storage instability problems such as coating delamination, crusting, and excessive precipitation during storage, and workability problems such as nozzle blockage due to high viscosity and obvious sagging of the paint film during spraying.
[0054] 2. The present invention further controls the compounding ratio of silicate compound, thickener, diethylene glycol butyl ether and alcohol ether solvent B, and introduces slow-drying modified polyol for matching, which not only prolongs the surface drying speed of the paint film, but also more accurately controls the drying time of the intermediate coating at 23°C 0.1s -1 The viscosity under low shear conditions is in the range of 50-65Pa.s with anti-sagging performance, 23℃250s -1 The viscosity under medium shear conditions is in the range of 170-210mPa.s, with good production dispersibility, 23℃1000s -1 The viscosity under high shear conditions is in the range of 100-130mPa.s, which has good spray fluidity, so that the mid-coat can further show good fluidity or anti-sagging performance both in the production stage and the construction stage. It is suitable for coating lines with long leveling time (more than 15 minutes) and maintains a good paint film appearance.
[0055] 3. The present invention adjusts the type of film-forming resin and matches appropriate polyurethane resin emulsion, acrylic emulsion and amino resin to make the entire paint film have better mechanical and chemical properties.
[0056] 4. The water-based intermediate coating of the present invention is suitable for coating situations where the leveling time is prolonged due to the modification of the process of the old 3C2B line. It not only saves the cost increase due to equipment modification, ensures that the old 3C2B line is not eliminated and can continue to operate normally, but also can obtain a composite paint film with excellent paint film appearance and meeting market requirements. DETAILED DESCRIPTION
[0057] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0058] The purpose of the present invention is illustrated by the following examples. The components of the composition are illustrated in parts by weight as a general standard. Unless otherwise specified, for the sake of simplicity, the "parts" described in the examples of the present invention have the same meaning as parts by weight.
[0059] According to one object of the present invention, the present invention discloses a water-based mid-coat for 3C1B1PH coating, comprising the following components in parts by weight:
[0060] 24-32 parts of polyurethane resin emulsion;
[0061] 2-4 parts of polyurethane resin;
[0062] 4-8 parts of water-based acrylic emulsion;
[0063] 5-7 parts of amino resin;
[0064] RD dispersion 4-10 parts;
[0065] 2.5-6.5 parts of additives;
[0066] 2.5-8 parts of alcohol ether solvent;
[0067] 20-30 parts water;
[0068] Wherein, the auxiliary agent comprises a thickener and a modified polyol; the RD dispersion comprises a silicate compound;
[0069] The mass ratio of the silicate compound, the thickener and the alcohol ether solvent is 0.12-0.3:1-2:2.5-8.
[0070] In the present invention, a water-based mid-coat with excellent anti-sagging performance is developed, which is suitable for a coating line with a long mid-coat leveling time. The purpose of designing the water-based mid-coat is that the existing 3C2B old line needs to be transformed into a 3C1B coating line to reduce coating costs and operating costs, but the cost of transforming the coating line and replacing the supporting equipment is huge, and it will also cause the original coating line to be stagnant during the transformation period, seriously affecting the normal operation of the coating company. In order to reduce the adverse effects caused by the transformation, the existing OEM factories usually change the operating procedures of the 3C2B old line, reduce the mid-coat pre-baking and baking operations, and replace them with continuing the mid-coat leveling. That is, after the car is sprayed with the mid-coat, only the leveling process is carried out without the mid-coat pre-baking and baking processes. The equipment for the mid-coat pre-baking and baking processes is shut down, so that the car is on the assembly line. Continue the leveling process. This method can achieve the change of coating process without modifying the assembly line, from 3C2B to 3C1B1PH. Although this solves the problem of assembly line modification, the extension of leveling time and the change of coating process (less pre-baking and baking) make the mid-coat that originally met the coating requirements no longer adapt to the new coating process, resulting in abnormal sagging or the surface of the paint film is dry but the inner layer is not dry. These problems will seriously affect the final appearance of the paint film. Therefore, it is necessary to solve the above problems from two aspects: enhancing the anti-sagging performance of the mid-coat and slowing down the surface drying speed of the paint film. At the same time, attention should be paid to viscosity control to ensure fluidity and construction operability during the production dispersion process.
[0071] First, the present invention reduces the surface drying speed of the paint film by introducing modified polyols and adjusting the type of alcohol ether solvents to match the longer leveling time. Specifically, the modified polyol uses slow-drying isotridecanol. According to a specific embodiment of the present invention, one or more of EXXAL 13TRIDECYL ALCOHOL of Mobil, isotridecanol of Hubei Rishengchang New Materials, and isotridecanol of Hubei Hengjingrui Chemical Co., Ltd. are selected, and the alcohol ether solvent is selected from one or more of ethylene glycol butyl ether, isooctyl alcohol, isopropanol, ethylene glycol hexyl ether, ethylene glycol isooctyl ether, and diethylene glycol butyl ether. However, it was later discovered that after the surface drying speed of the paint film was reduced, a longer leveling time would make abnormal sagging more likely to occur, so the anti-sagging performance requirements of the paint film would be higher.
[0072] On one hand, the present invention introduces RD dispersion (i.e. silicate compound thixotropic agent dispersion) and thickener to change the shear viscosity of the mid-coat, especially to improve the low shear viscosity, thereby improving the anti-sagging performance of the mid-coat.
[0073] Further, the thickener is selected from one or more of polyacrylate thickeners, polyurethane thickeners and polyamide wax thickeners; illustratively, the polyacrylate thickener is selected from one or more of BASF's Viscalex HV30, RHEOVIS AS 1130 and RHEOVIS HS 1152; the polyurethane thickener is selected from one or more of ADEKANOL UH-814N of ADEKA, 8W of Rohm and Haas and UCOAT N-800 of Sanyo; the polyamide wax thickener is selected from AQ-021 of Nanben Company.
[0074] Furthermore, RD dispersion is often used as a directing agent in topcoat and added to the formulation to improve the directivity of aluminum powder. In the present invention, RD dispersion is used as an auxiliary agent for improving low shear viscosity, and its composition includes a silicate compound, a polyether polyol and water. The RD dispersion is prepared by the following steps:
[0075] Under stirring conditions, 3 parts by weight of a silicate compound are slowly added to 60 parts by weight of water, followed by adding a total of 32 parts by weight of water in several times, stirring for 1-3 hours and then standing for at least 8 hours, then slowly adding 1.5 parts by weight of a polyether polyol and 3.5 parts by weight of water, stirring for 15-30 minutes, and standing for at least 8 hours again.
[0076] Furthermore, the polyether polyol is selected from one or more of PX-1000, PPG 1000, PPG 2000 and GP-1000 of Sanyo Chemical.
[0077] Furthermore, the silicate compound is a lithium magnesium silicate compound, selected from at least one of BYK's LaponiteRD, Hemmings' Hatorite RD or BYK's Optigel CG; in order to better provide efficient thixotropy and thermal stability of viscosity, it is necessary to further control the proportion of the silicate compound in the mid-coat. According to a specific implementation, the silicate compound accounts for 0.12%-0.3% of the total weight of the water-based mid-coat.
[0078] On the other hand, the present invention further improves the storage stability and workability of the coating by adjusting the compounding ratio of the silicate compound, the thickener and the alcohol ether solvent, so as to avoid storage instability problems such as coating delamination, skinning, and excessive precipitation during storage, and workability problems such as high viscosity blocking the nozzle and obvious sagging of the paint film during spraying. According to a specific embodiment of the present invention, the mass ratio of the silicate compound, the polyacrylate thickener and the alcohol ether solvent is 0.12-0.3:1-2:2.5-8, preferably 0.165:1.5:4.
[0079] Furthermore, the mass ratio of the silicate compound, the thickener, the alcohol ether solvent and the modified polyol is 0.12-0.3:1-2:2.5-8:0.2-0.5.
[0080] Furthermore, the mass ratio of the silicate compound, the thickener, the alcohol ether solvent and the modified polyol is 0.165:1.5:4:0.3.
[0081] In order to better meet the requirements of "wet-on-wet" coating, the inventors comprehensively considered various factors such as anti-sagging performance, paint film surface drying speed, viscosity and paint film appearance, and found that the introduction of diethylene glycol butyl ether would be more conducive to making the system meet the above requirements. Therefore, the alcohol ether solvent includes alcohol ether solvent A and alcohol ether solvent B; alcohol ether solvent A is mainly used to reduce the volatilization rate of the paint film and the wet film solid content, and alcohol ether solvent B is used to adjust the thixotropy of the system and the stability of the coating;
[0082] Among them, the alcohol ether solvent A is diethylene glycol butyl ether, which has the advantages of good water solubility, high boiling point, low volatilization rate, can reduce the volatilization rate, improve the pinhole limit, etc., and is suitable for the requirements of the present invention for long leveling time and good appearance of the paint film; the alcohol ether solvent B includes but is not limited to one or more of ethylene glycol butyl ether, isooctyl alcohol, isopropanol, ethylene glycol hexyl ether and ethylene glycol isooctyl ether.
[0083] Furthermore, the mass ratio of the silicate compound, thickener, alcohol ether solvent A, alcohol ether solvent B and modified polyol is 0.12-0.3:1-2:0.5-2:2-6:0.2-0.5. Preferably, when the mass ratio of the silicate compound, thickener, alcohol ether solvent A, alcohol ether solvent B and modified polyol is 0.165:1.5:1:3:0.3, such a compounding ratio can take into account the viscosity requirements of high, medium and low shear, so that it has moderate viscosity and certain fluidity during the production and dispersion process, has the characteristics of low viscosity under high-speed rotation of the rotary cup during the spraying process, and has the effect of high shear anti-sagging during the leveling process, specifically: it can not only prolong the surface drying speed of the paint film, but also more accurately control the 23°C 0.1s of the intermediate paint. -1 The viscosity under low shear conditions is in the range of 50-65Pa.s with anti-sagging performance, 23℃250s -1 The viscosity under medium shear conditions is in the range of 170-210mPa.s, with good production dispersibility, 23℃1000s -1 The viscosity under high shear conditions is in the range of 100-130mPa.s, which has good spray fluidity, so that the mid-coat can further show good fluidity or anti-sagging performance both in the production stage and the construction stage. It is suitable for coating lines with long leveling time (more than 15 minutes) and maintains a good paint film appearance.
[0084] Further, the polyurethane resin emulsion includes a wear-resistant polyurethane resin emulsion and / or a plasticized polyurethane emulsion. The wear-resistant polyurethane resin emulsion has good abrasion resistance and can provide the coating with excellent appearance, hardness, yellowing resistance, aging resistance and UV resistance. According to a specific embodiment of the present invention, the wear-resistant polyurethane resin emulsion is selected from one or more of ETERANE VK5516, ETERANE VK563 or ETERANE VK505 of Changxing Company; the plasticized polyurethane emulsion can work together with the RD dispersion used in the present invention to have stronger thixotropy. According to a specific embodiment of the present invention, the plasticized polyurethane emulsion is selected from one or more of DAOTAN TW 6466 / 36WA, DAOTAN TW 6431 / 45WA, and DAOTAN VTW 6462 / 36WA of Allnex.
[0085] Furthermore, the polyurethane resin emulsion comprises 20-24 parts by weight of wear-resistant polyurethane resin emulsion and 4-8 parts by weight of plasticizing polyurethane emulsion.
[0086] Furthermore, the polyurethane resin is a baking type polyurethane resin, which can undergo self-crosslinking reaction under baking conditions. The polyurethane resin provides the coating with good adhesion, flexibility and stone chip resistance, and has high reactivity and good pigment wettability and stability. According to a specific embodiment of the present invention, the polyurethane resin is selected from BAYHYTHERM 3246 and / or BAYHYTHERM 3146 of Bayer.
[0087] Furthermore, the aqueous acrylic emulsion can provide excellent physical and chemical properties for the coating. According to a specific embodiment of the present invention, the aqueous acrylic emulsion is selected from one or more of Setaqua 6803, Setaqua 6802 and Lacper 4702 of Allnex.
[0088] Further, the amino resin comprises a methyl etherified amino resin and / or an imino amino resin. According to a specific embodiment of the present invention, the methyl etherified amino resin is selected from one or more of CYMEL 303, CYMEL 308 and CYMEL350 of Allnex, and the methyl etherified amino resin has the characteristics of rapid crosslinking and slow self-polymerization; the imino amino resin is selected from one or more of CYMEL 325, CYMEL 327 and CYMEL 323 of Allnex, and the imino amino resin has high reactivity and has good hardness, gloss, chemical resistance and outdoor weather resistance after film formation.
[0089] Furthermore, the amino resin comprises 1-2 parts by weight of methyl etherified amino resin and 3-5 parts by weight of imino amino resin.
[0090] Furthermore, the additive further comprises 0.5-0.8 parts by weight of a dispersant, 1-3.5 parts by weight of a defoamer, 0.2-0.5 parts by weight of a wetting and leveling agent, 0.2-0.7 parts by weight of an anti-settling agent, 0.5-1.5 parts by weight of an orientation aid and 0.2-0.3 parts by weight of a pH adjuster.
[0091] Furthermore, the dispersant is selected from one or more of BYK-192, BYK-190 and BYK-180 produced by BYK Company.
[0092] Further, the defoamer can prevent a large number of bubbles from being generated during production and dispersion, and is selected from one or more of Evonik's tego805n, SURFYNOL 104A, SURFYNOL 104PG, BYK-WA, BYK-WS, BYK-OK. Among them, high-boiling-point olefin solvents such as BYK-WA, BYK-WS, BYK-OK of BYK can also prevent surface defects such as shrinkage cavities, orange peel, blistering, pinholes, etc., and prevent boiling marks to obtain excellent leveling properties.
[0093] Furthermore, the wetting and leveling agent is used to reduce surface tension and improve substrate wetting ability, and is selected from one or more of BYK-346, BYK-345 and BYK-347 produced by BYK.
[0094] Furthermore, the anti-precipitation agent refers to fumed silica, which has the function of preventing hard precipitation and is selected from one or more of AEROSIL R972, AEROSIL R974 and AEROSIL 200 of Evonik.
[0095] Furthermore, the directional aid is polyethylene wax, which has the characteristics of improving hardness and surface smoothness, and has the advantage of reducing short-wave defects (mottle, Bénard vortices). Exemplarily, the directional aid is selected from one or more of AQUACER 507, 532 or 526 of BYK.
[0096] Furthermore, the pH adjuster is dimethylethanolamine, which is used to adjust the pH value of the coating. Exemplarily, the pH adjuster is selected from dimethylacetamide produced by Shandong Jiawei Chemical Co., Ltd.
[0097] Furthermore, the water-based mid-coat paint also contains 20-25 parts by weight of titanium dioxide and 0-0.5 parts by weight of other commonly used pigments and fillers. For example, the titanium dioxide is selected from R-996 of Sichuan Longmang Titanium Industry Co., Ltd., and the other commonly used pigments and fillers include carbon black, iron red, iron yellow and other pigment powders, as well as fillers such as barium sulfate and talcum powder.
[0098] According to the second object of the present invention, the present invention discloses a method for preparing the water-based mid-coat as described above, comprising the following steps:
[0099] Under stirring conditions, a portion of the polyurethane resin emulsion, a portion of the alcohol ether solvent, a portion of the auxiliary agent, and a portion of water are mixed, the pH of the system is adjusted to 8.1-8.3, the premix viscosity is controlled to be 100-120 KU, and then the obtained mixture is sand-milled to obtain a sand-milled slurry;
[0100] Add the remaining polyurethane resin emulsion, polyurethane resin, water-based acrylic emulsion, amino resin, RD dispersion, remaining alcohol ether solvent, and remaining additives to the sand grinding slurry, mix well, adjust the system pH to 8.2-8.6, and then add water to adjust the viscosity to 180-200mPa.s (250s -1 , 23° C.), to obtain the water-based mid-coat paint.
[0101] Furthermore, the fineness of the sand grinding is controlled to be less than 10 μm.
[0102] According to the third object of the present invention, the present invention discloses an application of the water-based intermediate coating as described above in an automobile 3C1B1PH coating process.
[0103] Furthermore, the 3C1B1PH coating process is realized by shutting down the equipment for pre-baking and baking of the intermediate coating on the traditional 3C2B old line. Such a change makes the intermediate coating leveling time in the scheme of the present invention actually the sum of the time of the three steps (intermediate coating leveling, intermediate coating pre-baking and intermediate coating baking) of the previous 3C2B coating process, which indirectly prolongs the leveling time of the intermediate coating. The 3C1B1PH coating process of the present invention includes the following steps:
[0104] Sample electrophoresis treatment → spraying of mid-coat → mid-coat leveling → spraying of color paint → color paint leveling → color paint pre-baking → spraying of clear varnish → clear varnish leveling → clear varnish baking.
[0105] Furthermore, the paint film thickness of the intermediate paint is 12-14 μm.
[0106] Furthermore, the leveling time of the mid-coat is 15-20 minutes.
[0107] The technical solution of the present invention is described below in conjunction with some specific embodiments, wherein the reagents used in the embodiments include:
[0108] Polyurethane resin emulsion: ETERANE VK563 from Changxing, DAOTAN TW 6466 / 36WA from Allnex;
[0109] Polyurethane resin: BAYHYTHERM 3246 from Bayer;
[0110] Water-based acrylic emulsion: Setaqua 6803 from Allnex;
[0111] Amino resin: CYMEL 303 and CYMEL 325 from Allnex;
[0112] Polyacrylate thickener: Viscalex HV 30 from BASF;
[0113] Silicate compound: Laponite RD from BYK;
[0114] Isotridecyl alcohol: Mobil's EXXAL 13TRIDECYL ALCOHOL;
[0115] Polyether polyol: PX-1000 from Sanyo Chemical;
[0116] Dispersant: BYK-192 from BYK;
[0117] Defoamer: Evonik's tego 805n, BYK-WA from BYK;
[0118] Wetting and leveling agent: BYK-346 from BYK;
[0119] Directional additive: AQUACER 507 from BYK;
[0120] pH adjuster: dimethylacetamide from Shandong Jiawei Chemical Co., Ltd.;
[0121] Titanium dioxide: R-996 from Sichuan Longmang Titanium Industry Co., Ltd.;
[0122] Fumed silica: Evonik’s AEROSIL R972;
[0123] Ethylene glycol butyl ether: produced by Jiangsu Dena Chemical;
[0124] Diethylene glycol butyl ether: produced by Jiangsu Dena Chemical;
[0125] Isooctyl alcohol: produced by Tairong Chemical;
[0126] Iron red: BAYFERROX 130M from LANXESS;
[0127] Iron yellow: Bayferrox 3910 from LANXESS;
[0128] Carbon black: Degussa's Special Black 4.
[0129] Preparation Example: Preparation of RD Dispersion
[0130] Take a container and add 60 parts of water, turn on the stirring switch, and slowly add 3 parts of silicate compound while stirring at 300-500rpm. Increase the speed and stir for 40 minutes, then continue to add 12 parts of water, continue stirring for 60 minutes, take a sample and spray it on the polyester film to confirm that there are no spots, then add 20 parts of water and continue stirring for 60 minutes, let it stand for 8 hours, then add 1.5 parts of PX-1000 and 3.5 parts of water, continue stirring for 15 minutes, and then let it stand for another 8 hours, take a sample and spray it on the transparent polyester film to confirm that there are no spots, and then set aside. Control the temperature <45℃ throughout the process.
[0131] Examples 1-4
[0132] The specific water-based mid-coat paint formula disclosed in the present invention is shown in Table 1.
[0133] Table 1
[0134]
[0135]
[0136] The preparation process of mid-coat paint is as follows:
[0137] (1) Add raw materials 1 and 2 to container A and start stirring (speed is 200-300 rpm). After stirring for 15 minutes, use raw material 3 to adjust the pH value to 8.3-8.6;
[0138] (2) Add raw materials 4-7 to container B and start stirring (speed is 200-300 rpm). After stirring for 5 minutes, add the mixture in container B to container A. Continue stirring for 15 minutes and then use raw material 8 to adjust the pH value to 8.3-8.6;
[0139] (3) Take container C and add the mixed material in container A to container C, use raw material 9 to clean container A, add the washing liquid to container C, start stirring (speed is 200-300 rpm), stir for 15 minutes, add raw materials 10-14 in sequence under stirring, stir for 15 minutes and confirm that the stirring is uniform and there is no powder suspension surface, increase the speed to (speed is 600-800 rpm) and continue stirring for 60 minutes, then reduce the speed (speed is 400-500 rpm) and adjust the pH value to 8.1-8.3 with raw material 15, clean the cylinder wall and dispersion shaft with raw material 16, and adjust the viscosity to 100-120 KU (25°C);
[0140] Wherein, steps (1), (2) and (3) need to control the temperature at 20°C-40°C;
[0141] (4) using a sand mill to grind the mixed material in container C to a fineness of less than 10 μm to obtain a sand mill slurry, and using raw materials 17 and 18 to clean the sand mill, and the cleaning liquid is incorporated into the sand mill slurry;
[0142] The sand grinding conditions are as follows: using a water-based automobile-specific sand grinder, sand grinding method: PASS 4 times, fineness <10u; flow rate: 300±10KG / HR; sand grinding temperature ≤40°C;
[0143] (5) Calculate the sand grinding slurry yield and recalculate the subsequent input amount;
[0144] (6) Under stirring conditions (speed of 300-500 rpm), add raw materials 19-27 to the ground sand slurry in sequence (each material needs to be stirred for 10 minutes before adding the next material), then slowly add raw material 28 and continue stirring for 30 minutes;
[0145] (7) Add raw materials 29-31 into container D and stir for 15 minutes, then add to container C and the mixture in step (6) and stir for 30 minutes;
[0146] (8) Add raw materials 32-34 to container E and stir for 15 minutes, then add to container C and the mixture in step (7) and stir for 30 minutes;
[0147] (9) Add raw material 35-36 to container F and stir for 15 min. Then add it to container C and stir with the mixture in step (8) for 30 min.
[0148] (10) Use raw material 37 to adjust the pH value to 8.2-8.6, and use raw material 38 to adjust the viscosity to 180-200 mPa.s (250s -1 , 23℃), you’ll get it.
[0149] Board making process:
[0150] The water-based intermediate coating prepared in each embodiment is used for coating, and the coating process includes the following steps:
[0151] Sample electrophoresis treatment → spraying of intermediate coating → intermediate coating leveling → spraying of color paint → color paint leveling → color paint pre-baking → spraying of clear varnish → clear varnish leveling → clear varnish baking;
[0152] The film thickness of the intermediate coating is 12-14 μm; the leveling time of the intermediate coating is 15-20 min;
[0153] IPP 900 water-based A0A paint B2 (the paint used by Nippon Paint Daye Great Wall Factory) was used for paint spraying, with a film thickness of 10-14μm, leveling for 3 minutes, and pre-baking at 85℃ for 7 minutes;
[0154] CLEARCOAT PU 2K HD varnish (the paint used by Nippon Paint Taizhou Daye Factory) was selected for varnish spraying, with a film thickness of 50-60μm, leveling for 7 minutes, and baking at 145℃ for 25 minutes.
[0155] The spray room temperature is 22-24°C, the humidity is 62-68% RH, and the equipment parameters of the spray robot are shown in Table 2:
[0156] Table 2
[0157]
[0158]
[0159] The test methods and results of the obtained coatings are summarized in Table 5.
[0160] Comparative Examples 1-7
[0161] The specific water-based mid-coat paint formula table disclosed in the comparative example is shown in Table 3.
[0162] Table 3
[0163]
[0164]
[0165] The preparation process of mid-coat paint is as follows:
[0166] (1) Add raw materials 1 and 2 to container A and start stirring (speed is 200-300 rpm). After stirring for 15 minutes, use raw material 3 to adjust the pH value to 8.3-8.6;
[0167] (2) Add raw materials 4-7 to container B and start stirring (speed is 200-300 rpm). After stirring for 5 minutes, add the mixture in container B to container A. Continue stirring for 15 minutes and then use raw material 8 to adjust the pH value to 8.3-8.6;
[0168] (3) Take container C and add the mixed material in container A to container C, use raw material 9 to clean container A, add the washing liquid to container C, start stirring (speed is 200-300 rpm), stir for 15 minutes, add raw materials 10-14 in sequence under stirring, stir for 15 minutes and confirm that the stirring is uniform and there is no powder suspension surface, increase the speed to (speed is 600-800 rpm) and continue stirring for 60 minutes, then reduce the speed (speed is 400-500 rpm) and adjust the pH value to 8.1-8.3 with raw material 15, clean the cylinder wall and dispersion shaft with raw material 16, and adjust the viscosity to 100-120 KU (25°C);
[0169] Wherein, steps (1), (2) and (3) need to control the temperature at 20°C-40°C;
[0170] (4) using a sand mill to grind the mixed material in container C to a fineness of less than 10 μm to obtain a sand mill slurry, and using raw materials 17 and 18 to clean the sand mill, and the cleaning liquid is incorporated into the sand mill slurry;
[0171] The sand grinding conditions are as follows: using a water-based automobile-specific sand grinder, sand grinding method: PASS 4 times, fineness <10u; flow rate: 300±10KG / HR; sand grinding temperature ≤40°C;
[0172] (5) Calculate the sand grinding slurry yield and recalculate the subsequent input amount;
[0173] (6) Under stirring conditions (speed of 300-500 rpm), add raw materials 19-27 to the ground sand slurry in sequence (each material needs to be stirred for 10 minutes before adding the next material), then slowly add raw material 28 and continue stirring for 30 minutes;
[0174] (7) Add raw materials 29-31 into container D and stir for 15 minutes, then add to container C and the mixture in step (6) and stir for 30 minutes;
[0175] (8) Add raw materials 32-34 to container E and stir for 15 minutes, then add to container C and the mixture in step (7) and stir for 30 minutes;
[0176] (9) Add raw material 35-36 to container F and stir for 15 min. Then add it to container C and stir with the mixture in step (8) for 30 min.
[0177] (10) Use raw material 37 to adjust the pH value to 8.2-8.6, and use raw material 38 to adjust the viscosity to 180-200 mPa.s (250s -1 , 23℃), you’ll get it.
[0178] Board making process:
[0179] The water-based intermediate coating prepared in each embodiment is used for coating, and the coating process includes the following steps:
[0180] Sample electrophoresis treatment → spraying of intermediate coating → intermediate coating leveling → spraying of color paint → color paint leveling → color paint pre-baking → spraying of clear varnish → clear varnish leveling → clear varnish baking;
[0181] The film thickness of the intermediate coating is 12-14 μm; the leveling time of the intermediate coating is 15-20 min;
[0182] IPP 900 water-based A0A paint B2 (the paint used by Nippon Paint Daye Great Wall Factory) was used for paint spraying, with a film thickness of 10-14μm, leveling for 3 minutes, and pre-baking at 85℃ for 7 minutes;
[0183] CLEARCOAT PU 2K HD varnish (the paint used by Nippon Paint Taizhou Daye Factory) was selected for varnish spraying, with a film thickness of 50-60μm, leveling for 7 minutes, and baking at 145℃ for 25 minutes.
[0184] The spray room temperature is 22-24°C, the humidity is 62-68% RH, and the equipment parameters of the spray robot are shown in Table 4:
[0185] Table 4
[0186] Atomizer Model DURR Hanging cup speed / rpm 4.5W Gun distance / mm 200 <![CDATA[Muzzle velocity / m·s -1 > 0.45 Molding air / mL·min 250 Interval / mm 100 Flow rate / mL·min 200 Current / μA 350
[0187] The samples prepared from Examples 1-4 and Comparative Examples 1-7 were tested, and the test methods and results are as follows:
[0188] Table 5
[0189]
[0190]
[0191] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.
Claims
1. A water-based mid-coat for 3C1B1PH coating, characterized in that: Contains the following components in parts by weight: 24-32 parts of polyurethane resin emulsion; 2-4 parts of polyurethane resin; 4-8 parts of water-based acrylic emulsion; 5-7 parts of amino resin; RD dispersion 4-10 parts; 2.5-6.5 parts of additives; 2.5-8 parts of alcohol ether solvent; 20-30 parts water; Wherein, the auxiliary agent comprises a thickener and a modified polyol; the RD dispersion comprises a silicate compound; The mass ratio of the silicate compound, the thickener and the alcohol ether solvent is 0.12-0.3:1-2:2.5-8.
2. The water-based mid-coat paint according to claim 1, characterized in that: The mass ratio of the silicate compound, the thickener, the alcohol ether solvent and the modified polyol is 0.12-0.3:1-2:2.5-8:0.2-0.5; Preferably, the mass ratio of the silicate compound, the thickener, the alcohol ether solvent and the modified polyol is 0.165:1.5:4:0.
3.
3. The water-based mid-coat paint according to claim 1, characterized in that: The thickener is selected from one or more of polyacrylate thickeners, polyurethane thickeners and polyamide wax thickeners; The modified polyol is isotridecanol.
4. The water-based mid-coat paint according to claim 1, characterized in that: The alcohol ether solvent comprises an alcohol ether solvent A and an alcohol ether solvent B; Wherein, the alcohol ether solvent A is diethylene glycol butyl ether, and the alcohol ether solvent B is selected from one or more of ethylene glycol butyl ether, isooctyl alcohol, isopropanol, ethylene glycol hexyl ether and ethylene glycol isooctyl ether; Preferably, the mass ratio of the silicate compound, the thickener, the alcohol ether solvent A, the alcohol ether solvent B and the modified polyol is 0.12-0.3:1-2:0.5-2:2-6:0.2-0.5; More preferably, the mass ratio of the silicate compound, the thickener, the alcohol ether solvent A, the alcohol ether solvent B and the modified polyol is 0.165:1.5:1:3:0.
3.
5. The water-based mid-coat paint according to claim 1, characterized in that: The polyurethane resin emulsion comprises a wear-resistant polyurethane resin emulsion and / or a plasticized polyurethane emulsion; Preferably, the polyurethane resin emulsion comprises 20-24 parts by weight of wear-resistant polyurethane resin emulsion and 4-8 parts by weight of plasticizing polyurethane emulsion; Preferably, the wear-resistant polyurethane resin emulsion is selected from one or more of ETERANE VK5516, ETERANE VK563 and ETERANE VK505 of Changxing Company; Preferably, the plasticized polyurethane emulsion is selected from one or more of DAOTAN TW 6466 / 36WA, DAOTAN TW6431 / 45WA and DAOTAN VTW 6462 / 36WA of Allnex.
6. The water-based mid-coat paint according to claim 1, characterized in that: The amino resin comprises a methyl etherified amino resin and / or an imino amino resin; Preferably, the amino resin comprises 1-2 parts by weight of methyl etherified amino resin and 3-5 parts by weight of imino amino resin; Preferably, the methyl etherified amino resin is selected from one or more of CYMEL 303, CYMEL 308 and CYMEL 350 of Allnex; Preferably, the iminoamino resin is selected from one or more of CYMEL 325, CYMEL 327 and CYMEL 323 of allnex.
7. The water-based mid-coat paint according to claim 1, characterized in that: The RD dispersion is prepared by the following steps: Under stirring conditions, 3 parts by weight of a silicate compound is slowly added to 60 parts by weight of water, and then a total of 32 parts by weight of water is added in multiple times, stirred for 1-3 hours, and then allowed to stand for at least 8 hours, and then 1.5 parts by weight of a polyether polyol and 3.5 parts by weight of water are slowly added, and then stirred for 15-30 minutes, and allowed to stand for at least 8 hours again, to obtain; Preferably, the silicate compound is selected from one or more of Laponite RD of BYK, Hatorite RD of Hemmings and Optigel CG of BYK; the silicate compound accounts for 0.12%-0.3% of the total weight of the water-based mid-coat; Preferably, the polyether polyol is selected from one or more of PX-1000, PPG 1000, PPG 2000 and GP-1000 of Sanyo Chemical.
8. The water-based mid-coat paint according to claim 1, characterized in that: The water-based mid-coat paint further comprises 20-25 parts by weight of titanium dioxide and 0-0.5 parts by weight of other pigments and fillers; The other pigments and fillers are selected from one or more of carbon black, iron red, iron yellow, barium sulfate and talc.
9. The method for preparing a water-based mid-coat paint according to any one of claims 1 to 8, characterized in that: The steps include: Under stirring conditions, a portion of the polyurethane resin emulsion, a portion of the alcohol ether solvent, a portion of the auxiliary agent, and a portion of water are mixed, the pH of the system is adjusted to 8.1-8.3, the premix viscosity is controlled to be 100-120 KU, and then the obtained mixture is sand-milled to obtain a sand-milled slurry; Add the remaining polyurethane resin emulsion, polyurethane resin, water-based acrylic emulsion, amino resin, RD dispersion, the remaining alcohol ether solvent, and the remaining additives to the sand-polished slurry, mix well, adjust the system pH to 8.2-8.6, and then add water to adjust the viscosity to 180-200 mPa.s to obtain the water-based mid-coat paint.
10. The use of the water-based mid-coat paint according to any one of claims 1 to 8 in a 3C1B1PH coating process for automobiles, characterized in that: The 3C1B1PH coating process includes the following steps: Sample electrophoresis treatment → spraying of intermediate coating → intermediate coating leveling → spraying of color paint → color paint leveling → color paint pre-baking → spraying of clear varnish → clear varnish leveling → clear varnish baking; Preferably, the paint film thickness of the intermediate paint is 12-14 μm; Preferably, the leveling time of the intermediate coating is 15-20 minutes.