Silicon carbide polishing solution as well as preparation method and application thereof
By introducing a mixed abrasive of organic abrasives with alumina or zirconium oxide into the silicon carbide polishing liquid, combining oxidants and catalysts, the scratches and roughness problems caused by alumina abrasives are solved, and the polishing quality of silicon carbide wafers is improved and Speed simplifies processing process.
Patent Information
- Application Number
- CN202411129557.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
Alumina or zirconium oxide abrasives in existing silicon carbide polishing liquids can easily cause scratches and high surface roughness, affecting the processing efficiency of silicon carbide wafers.
Organic abrasives are introduced on the basis of alumina or zirconia abrasives to form mixed abrasives, combined with oxidants, catalysts and pH regulators, reduce scratches and roughness through chemical mechanical polishing technology, and optimize the composition and process parameters of the polishing liquid.
It effectively reduces scratches during the polishing process, reduces surface roughness, improves polishing quality and rate, and simplifies the subsequent finishing processing process.
Smart Images

Figure BDA0004997427670000071 
Figure FDA0004997427660000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polishing materials, and particularly relates to a silicon carbide polishing liquid and a preparation method and application thereof. Background Art
[0002] SiC is the main third-generation semiconductor material. Compared with single crystal materials such as the first-generation semiconductor Si and the second-generation semiconductor GaAs, SiC crystals have the characteristics of large bandgap width, high thermal conductivity, large electron saturation drift rate, high critical breakdown electric field, low dielectric constant, and good chemical stability. It has broad application prospects in high-frequency, high-power, high-temperature resistant, radiation-resistant semiconductor devices, ultraviolet detectors, and short-wave light-emitting diodes. Devices made of it can be used at high temperatures above 600°C. SiC crystals are made of densely packed SiC tetrahedrons. Due to different stacking methods, SiC has more than 200 different crystal forms, but only a few such as 3C, 2H, 4H, 6H, and 15R can exist stably. Silicon carbide semiconductors conform to the overall model of the industrial chain. Through the combination of silicon carbide raw materials, crystals, substrates, epitaxy, chips, and modules, the presentation of silicon carbide semiconductors is completed, which conforms to the application of industrial development models. The growth of silicon carbide single crystals conforms to the device standard content of silicon carbide. Through effective composition and hot spot model development analysis, the development trend effect is expanded to achieve effective silicon carbide single crystal applications. Due to the high hardness of single-crystal silicon carbide, the processing of single-crystal silicon carbide wafers has always been a difficult problem. The processing of silicon carbide wafers is mainly achieved through coarse and fine diamond liquid grinding to achieve the purpose of rapid thinning, and then through ultra-coarse and fine polishing to obtain a perfect surface.
[0003] Chemical Mechanical Polishing (CMP) is the only means to achieve global flatness in integrated circuit manufacturing. This process is specially designed to obtain a surface that is flat and free of scratches and impurities. CMP is a technology that combines chemical and mechanical actions. Its process is quite complicated and has many influencing factors. First, the surface material of the workpiece reacts chemically with the oxidant, catalyst, etc. in the polishing liquid to form a relatively easy-to-remove soft layer. Then, the soft layer is removed under the mechanical action of the abrasive and polishing pad in the polishing liquid, exposing the surface of the workpiece again. Then, a chemical reaction is carried out. In this way, the surface polishing of the workpiece is completed in the alternation of chemical and mechanical processes. The polishing liquid plays a key role in chemical mechanical polishing.
[0004] Currently, silicon carbide polishing fluid mainly uses superhard materials such as aluminum oxide or zirconium oxide as abrasives, but this type of polishing fluid can easily cause scratches and excessive roughness on the surface. Summary of the invention
[0005] In view of the defects of the prior art, the technical problem to be solved by the present invention is to provide a silicon carbide polishing liquid and its preparation method and application, so as to solve the problems of high scratches and large roughness of pure aluminum oxide abrasives in the prior art. The present invention mainly introduces organic abrasives on the basis of superhard abrasives such as aluminum oxide or zirconium oxide to form mixed abrasives, further reducing scratches and roughness, and further shortening the efficiency of the subsequent fine polishing process.
[0006] The present invention provides a polishing liquid, which comprises, by weight percentage:
[0007] The abrasives include superhard abrasives and organic abrasives.
[0008] Preferably, the liquid carrier is water;
[0009] The superhard abrasive and the organic abrasive are mixed in any proportion.
[0010] Preferably, the abrasive comprises 0.5-10% superhard abrasive and 0.5-5% organic abrasive;
[0011] Preferably, the super-hard abrasive comprises one or more of aluminum oxide and zirconium oxide, preferably aluminum oxide; the particle size of the super-hard abrasive is 5 nm-2 μm, preferably 60 nm-0.5 μm, and most preferably 100 nm-0.3 μm.
[0012] Preferably, the organic abrasive is a microsphere formed by a polymer, and the particle size of the organic abrasive is in the range of 50 nm-5 μm, preferably between 100 nm-2 μm, and most preferably between 0.5 μm-1 μm.
[0013] Preferably, the microspheres formed by the polymer include plastic microspheres, synthetic rubber microspheres, and synthetic fiber microspheres.
[0014] Preferably, the plastic microspheres include one or more of polystyrene ball mills, polyethylene ball mills, and polypropylene ball mills.
[0015] Preferably, the synthetic rubber microspheres include one or more of styrene-butadiene rubber microspheres, nitrile-butadiene rubber microspheres, and isoprene rubber microspheres.
[0016] Preferably, the synthetic fiber microspheres include one or more of nylon microspheres, polyester microspheres, acrylic microspheres, polypropylene microspheres, and vinylon microspheres.
[0017] More preferably, the organic abrasive is nylon microspheres.
[0018] Preferably, the oxidant is one or more of an organic oxidant and an inorganic oxidant.
[0019] Preferably, the inorganic oxidant comprises chlorate: ClO3 - , Perchlorate: ClO4 - , Inorganic peroxides, Nitrates: NO3 - 、Permanganate MnO4 - , ferrate FeO4 2- 、Metal cations such as Fe 3+ , Cu 2+ etc., one or more of sodium perborate, potassium perborate, chloric acid, chlorous acid, chloric acid, perchloric acid, bromic acid, perbromic acid, iodic acid, periodic acid, hypochlorite, chlorite, bromate, perbromate, iodate, and periodate.
[0020] The inorganic peroxide includes one or more of Na2O2, K2O2, MgO2, CaO2, BaO2, and H2O2.
[0021] Preferably, the organic oxidant comprises one or more of peracetic acid, performic acid, dicumyl peroxide, benzoyl peroxide, methyl ethyl ketone peroxide, cyclohexanone peroxide, tert-butyl peroxide, tert-butyl perbenzoate, peracetic acid, monoperoxyphthalic acid, peroxytrifluoroacetic acid, peroxym-chlorobenzoic acid, peroxybenzoic acid, and peroxyp-nitrobenzoic acid.
[0022] Furthermore, the oxidant is preferably potassium permanganate or sodium permanganate, and most preferably potassium permanganate.
[0023] The pH stabilizer is slightly different from the buffer. The alkaline stabilizer in this experiment is the hydrolysis of the cations in the strong acid and weak base salt to stabilize the alkalinity. It should be emphasized here that different cations are stable in different pH ranges. The pH range here is the pH after the corresponding strong acid and weak base salt is dissolved in pure water, which is within a limited range above and below this pH value. The acidic stabilizer in this experiment is the hydrolysis of the anions in the strong base and weak base salt to stabilize the acidity. It should be emphasized here that different anions are also stable in different pH ranges. The pH range here is the pH after the corresponding strong base and weak base salt is dissolved in pure water, which is within a limited range above and below this pH value.
[0024] Preferably, the pH stabilizer includes one or more of an alkaline stabilizer and an acidic stabilizer.
[0025] Preferably, the alkaline stabilizer is a strong acid weak base salt, wherein the cation in the strong acid weak base salt is Cu 2+ (such as copper nitrate, copper chloride, copper sulfate), Al 3+ (such as aluminum nitrate, aluminum sulfate, aluminum chloride), Fe 3+ (such as ferric nitrate, ferric sulfate, ferric chloride), Zn 2+ (zinc nitrate, zinc chloride, zinc sulfate), Ni2+ (nickel nitrate, nickel sulfate, nickel chloride) one or more.
[0026] Preferably, the acidic stabilizer is a strong base weak acid salt, wherein the strong base weak acid salt includes one or more of potassium silicate, sodium silicate, lithium silicate, sodium phosphate, potassium phosphate, sodium aluminate, potassium aluminate, sodium aluminate, potassium aluminate, sodium borate, potassium borate, sodium arsenate, potassium arsenate, sodium selenate, potassium selenate, sodium tellurate, and sodium tellurate.
[0027] Preferably, the strong acid and weak base salt includes one or more of copper nitrate, copper chloride, copper sulfate, aluminum nitrate, aluminum sulfate, aluminum chloride, ferric nitrate, ferric sulfate, ferric chloride, zinc nitrate, zinc chloride, zinc sulfate, nickel nitrate, nickel sulfate, and nickel chloride.
[0028] Preferably, the pH adjuster is one or more of potassium hydroxide solution and nitric acid solution, and the pH range is preferably 2.00-13.50.
[0029] Preferably, the silicon carbide polishing liquid further comprises 0.01-0.1% of a dispersant.
[0030] Preferably, the dispersant (agent for inhibiting the crystallization of silica sol) includes one or more of polyhydroxy organic matter, ketone organic matter, and ether organic matter;
[0031] Preferably, the polyhydroxy organic matter includes one or more of glycerol, cellulose, glucose, sucrose, fructose, ethylene glycol, and starch; the ketone organic matter includes one or more of aliphatic ketones, alicyclic ketones, aromatic ketones, saturated ketones, and unsaturated ketones; the ether organic matter includes ether, which is a product in which the hydrogen in the hydroxyl group of alcohol or phenol is replaced by a hydrocarbon group, and the general formula is RO-R', wherein R is a saturated fatty chain; the R' is a saturated fatty chain, and R and R' may be the same or different.
[0032] The dispersant is used to reduce the crystallization of silica sol particles, because the crystals are easy to adhere to the surface of the pad, and micro scratches are easy to occur during the polishing process, thereby causing the local roughness to be too high.
[0033] Preferably, the silicon carbide polishing liquid also includes 0.01-5% of a catalyst; the catalyst includes HgCl2, KI, Fe 2+ , rhodium monophosphine water-soluble catalysts such as TPPTS / Rh, rhodium diphosphine water-soluble catalysts such as BISBIS / Rh, hydrazine hydrate, triphenylphosphine tris-sulfonic acid sodium salt, rhodium chloride, p-toluenesulfonic acid, water-soluble organic molybdenum salts, pyridine or imidazole ionic liquids, dichlorodi(1,10-phenanthroline), ammonium molybdate, Cu-polyamide amine complex, Mn-polyamide amine complex, sodium metavanadate, sodium vanadate, InVO4, Cr(VI) or more thereof.
[0034] The function of the catalyst is to accelerate the reaction between the oxidant and silicon carbide. The catalyst directly or indirectly participates in the reaction process between the oxidant and silicon carbide.
[0035] The present invention provides a method for preparing a silicon carbide polishing liquid, comprising:
[0036] The components are weighed according to weight percentage, the superhard abrasive and the organic abrasive are mixed, and then mixed with other components except the pH adjuster, and then the pH value is adjusted with the pH adjuster to obtain the silicon carbide polishing liquid.
[0037] The present invention provides an application of the polishing liquid in polishing a silicon carbide material, wherein the silicon carbide material is one or more of an insulating silicon carbide wafer, a doped silicon carbide wafer (N-type silicon carbide or P-type silicon carbide), and a silicon carbide film. The crystal form of the silicon carbide wafer can be 3C-SiC, 4H-SiC, 6H-SiC, or other stable crystal forms.
[0038] The present invention provides a polishing method using any of the polishing liquids, comprising: adhering a silicon carbide material to a polishing head, and polishing the silicon carbide material using the polishing liquid of any of claims 1-8.
[0039] The silicon carbide material is one or more of an insulating silicon carbide wafer, a doped silicon carbide wafer, and a silicon carbide film; the polishing process parameters include: polishing pressure of 3-6psi; polishing pad speed of 50-110rpm; polishing sheet speed of 50-110rpm; polishing liquid flow rate of 30-130mL / min for circulation; and polishing time of 15min-3h.
[0040] Beneficial Effects
[0041] The present invention provides a new method for preparing a silicon carbide polishing liquid, which overcomes the shortcomings of the prior art and has a simple and efficient preparation method. In addition, by adding different organic abrasives to the polishing liquid, the polishing quality (including crystallization performance), polishing rate and polishing surface of the polishing liquid are also greatly improved. DETAILED DESCRIPTION
[0042] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0043] Example 1
[0044] Mix super-hard abrasive (aluminum oxide or zirconium oxide) with different organic abrasives, and optionally add oxidants, catalysts, dispersants, and pH stabilizers. Then use potassium hydroxide to adjust the pH of the polishing liquid to 9-10, stir evenly and prepare for polishing.
[0045] A: 5wt% 0.3um Al2O3+1wt% 0.5um nylon microspheres+2.5wt% KMnO4+0.1wt% potassium phosphate+
[0046] 0.05wt%KOH+91.35wt%water;
[0047] B: 5wt% 0.3umAl2O3+1wt% 0.5um polyethylene microspheres+2.5wt% KMnO4+0.1wt% potassium phosphate+
[0048] 0.05wt%KOH+91.35wt%water;
[0049] C: 5wt% 0.3um Al2O3 + 1wt% 0.5um styrene-butadiene rubber microspheres + 2.5wt% KMnO4 + 0.1wt% potassium phosphate +
[0050] 0.05wt%KOH+91.35wt%water;
[0051] D: 5wt% 0.3umAl2O3+1wt% 0.5um polyvinyl chloride microspheres+2.5wt% KMnO4+0.1wt% potassium phosphate+
[0052] 0.05wt%KOH+91.35wt%water;
[0053] E: 5wt% 0.3um Al2O3 + 1wt% 0.5um acrylic microspheres + 2.5wt% KMnO4 + 0.1wt% potassium phosphate +
[0054] 0.05wt%KOH+91.35wt%water;
[0055] F: 5wt% 0.3um ZrO2 + 1wt% 0.5um nylon microspheres + 2.5wt% KMnO4 + 0.1wt% potassium phosphate +
[0056] 0.05wt%KOH+91.35wt%water;
[0057] G: 5wt% 0.3um ZrO2 + 1wt% 0.5um polyethylene microspheres + 2.5wt% KMnO4 + 0.1wt% potassium phosphate +
[0058] 0.05wt%KOH+91.35wt%water;
[0059] H: 5wt% 0.3um ZrO2+1wt% 0.5um styrene-butadiene rubber microspheres+2.5wt% KMnO4+0.1wt% potassium phosphate
[0060] + 0.05wt% KOH + 91.35wt% water;
[0061] I: 5wt% 0.3um ZrO2 + 1wt% 0.5um polyvinyl chloride microspheres + 2.5wt% KMnO4 + 0.1wt% potassium phosphate +
[0062] 0.05wt%KOH+91.35wt%water;
[0063] J: 5wt% 0.3um ZrO2 + 1wt% 0.5um acrylic microspheres + 2.5wt% KMnO4 + 0.1wt% potassium phosphate +
[0064] 0.05wt%KOH+91.35wt%water;
[0065] K: 5wt% 0.3umAl2O3 + 2.5wt% KMnO4 + 0.1wt% potassium phosphate + 0.05wt% KOH + 92.4wt% water;
[0066] L: 5wt% 0.3um ZrO2+2.5wt% KMnO4+0.1wt% potassium phosphate+0.05wt% KOH+92.4wt% water;
[0067] Polishing experiment: This polishing experiment uses a CP-4 machine, and a 4-inch silicon carbide wafer (semi-insulating, Si surface) is glued to the polishing head through wax. The polishing parameters are set as follows: SUBA800 polishing pad; polishing pressure is 6psi; polishing pad speed is 100rpm; polishing sheet speed is 90rpm; polishing liquid flow rate is 125mL / min for recycling; polishing time is 60min. After each polishing, the polishing pad is repaired for 5 minutes with a 4-inch diamond repair disk, and the polished sheet is ultrasonically cleaned in the cleaning solution for 10 minutes and then blown dry with nitrogen. The results are listed in Table 1.
[0068] Table 1: Experimental results statistics
[0069] Experimental samples Polishing rate (um / h) Total scratch length / mm Ra / nm A 1.31 15 0.114 B 1.18 35 0.115 C 1.05 30 0.119 D 1.11 27 0.110 E 1.17 45 0.119 F 1.25 18 0.118 G 1.05 21 0.115 H 1.03 27 0.108 I 1.07 20 0.118 J 1.00 29 0.120 K 1.21 57 0.126 L 1.15 53 0.124
[0070] Conclusion: The introduction of organic abrasives effectively reduces the total length of scratches and significantly reduces the surface roughness Ra. Among them, nylon microspheres effectively increase the removal rate and the surface improvement is the most obvious.
[0071] Example 2
[0072] Mix super-hard abrasives - aluminum oxide of different particle sizes and different contents with organic abrasives of different particle sizes, and add oxidants, catalysts, dispersants, and pH stabilizers. Use dilute potassium hydroxide or dilute nitric acid to adjust the pH of the polishing liquid to 9-10, and stir evenly for polishing.
[0073] Polishing experiment: This polishing experiment uses a CP-4 machine, and a 4-inch silicon carbide wafer (semi-insulating, Si surface) is glued to the polishing head through wax. The polishing parameters are set as follows: SUBA800 polishing pad; polishing pressure is 6psi; polishing pad speed is 100rpm; polishing sheet speed is 90rpm; polishing liquid flow rate is 125mL / min for recycling; polishing time is 60min. After each polishing, the polishing pad is repaired for 5 minutes with a 4-inch diamond repair disk, and the polished sheet is ultrasonically cleaned in the cleaning liquid for 10 minutes and then blown dry with nitrogen. The results are listed in Table 2.
[0074] 1.5wt% 0.3umAl2O3+0.5wt% 0.5um nylon microspheres+2.5wt% KMnO4+0.1wt% potassium phosphate+0.05wt% KOH+91.85wt% water;
[0075] 2.5wt% 0.3umAl2O3+1.5wt% 0.5um nylon microspheres+2.5wt% KMnO4+0.1wt% potassium phosphate+0.05wt% KOH+90.35wt% water;
[0076] 3.5wt% 0.3um Al2O3+1wt% 2um nylon microspheres+2.5wt% KMnO4+0.1wt% potassium phosphate+0.05wt% KOH+90.85wt% water;
[0077] 4.5wt% 0.1umAl2O3+1wt% 0.5um nylon microspheres+2.5wt% KMnO4+0.1wt% potassium phosphate+0.05wt% KOH+90.85wt% water;
[0078] 5.5wt% 0.15umAl2O3+1wt% 0.5um nylon microspheres+2.5wt% KMnO4+0.1wt% potassium phosphate+0.05wt% KOH+90.85wt% water;
[0079] 6.5wt% 0.5umAl2O3+1wt% 0.5um nylon microspheres+2.5wt% KMnO4+0.1wt% potassium phosphate+0.05wt% KOH+90.85wt% water;
[0080] 7.5wt% 2umAl2O3+1wt% 0.5um nylon microspheres+2.5wt% KMnO4+0.1wt% potassium phosphate+0.05wt% KOH+90.85wt% water;
[0081] 8.5wt% 0.15um Al2O3+1wt% 0.5um nylon microspheres+2.5wt% KMnO4+0.1wt% ferric nitrate+0.1wt% acetic acid+91.3wt% water, pH=2.5;
[0082] 9.5wt% 0.15um Al2O3+1wt% 0.5um nylon microspheres+3.5wt% KMnO4+0.1wt% copper nitrate+0.1wt% silicic acid+90.3wt% water; pH=2.5;
[0083] 10.5wt% 0.15um Al2O3+1wt% 0.5um nylon microspheres+2.5wt% KMnO4+0.1wt% nickel nitrate+0.1wt% acetone+0.05wt% KOH+91.25wt% water; pH=9-10;
[0084] 11.5wt% 0.15um Al2O3+1wt% 0.5um nylon microspheres+2.5wt% KMnO4+0.1wt% nickel nitrate+0.1wt% cellulose+0.05wt% KOH+91.25wt% water; pH=9-10.
[0085] Table 2: Experimental results statistics
[0086]
[0087]
[0088] In summary, the present invention effectively overcomes various shortcomings of the prior art and has high industrial utilization value.
Claims
1. A polishing liquid, characterized in that: By weight percentage, the components include: The abrasives include superhard abrasives and organic abrasives.
2. The polishing liquid according to claim 1, characterized in that: The liquid phase carrier is water; The abrasive material comprises 0.5-10% superhard abrasive and 0.5-5% organic abrasive; The super-hard abrasive comprises one or more of aluminum oxide and zirconium oxide; the particle size of the super-hard abrasive is 5nm-2μm; the organic abrasive is a microsphere formed by a polymer, and the particle size of the organic abrasive ranges from 50nm-5μm.
3. The polishing liquid according to claim 2, characterized in that: The microspheres formed by the polymer include plastic microspheres, synthetic rubber microspheres, and synthetic fiber microspheres; The plastic microspheres include one or more of polystyrene ball abrasives, polyethylene ball abrasives, and polypropylene ball abrasives; The synthetic rubber microspheres include one or more of styrene-butadiene rubber microspheres, nitrile rubber microspheres, and isoprene rubber microspheres; the synthetic fiber microspheres include one or more of nylon microspheres, polyester microspheres, acrylic microspheres, polypropylene microspheres, and vinylon microspheres.
4. The polishing liquid according to claim 1, characterized in that: The oxidant is one or more of an organic oxidant and an inorganic oxidant; The inorganic oxidant comprises one or more of chlorate, perchlorate, inorganic peroxide, nitrate, permanganate, ferrate, sodium perborate, potassium perborate, chloric acid, chlorous acid, chloric acid, perchloric acid, bromic acid, perbromic acid, iodic acid, periodic acid, hypochlorite, chlorite, bromate, perbromate, iodate, periodate, and metal cations; wherein the inorganic peroxide comprises one or more of Na2O2, K2O2, MgO2, CaO2, BaO2, and H2O2; The organic oxidant includes one or more of peracetic acid, performic acid, dicumyl peroxide, benzoyl peroxide, methyl ethyl ketone peroxide, cyclohexanone peroxide, tert-butyl peroxide, tert-butyl perbenzoate, peracetic acid, monoperoxyphthalic acid, peroxytrifluoroacetic acid, peroxym-chlorobenzoic acid, peroxybenzoic acid, and peroxyp-nitrobenzoic acid.
5. The polishing liquid according to claim 1, characterized in that: The pH stabilizer includes one or more of an alkaline stabilizer and an acidic stabilizer; The alkaline stabilizer is a strong acid weak base salt, wherein the cation in the strong acid weak base salt is Cu 2+ 、Al 3+ , Fe 3+ 、Zn 2+ 、Ni 2+ One or more of the following; The acidic stabilizer is a strong base weak acid salt, wherein the strong base weak acid salt includes one or more of potassium silicate, sodium silicate, lithium silicate, sodium phosphate, potassium phosphate, sodium metaaluminate, potassium metaaluminate, sodium aluminate, potassium aluminate, sodium borate, potassium borate, sodium arsenate, potassium arsenate, sodium selenate, potassium selenate, sodium tellurate, and sodium tellurate.
6. The polishing liquid according to claim 5, characterized in that: The strong acid and weak base salt includes one or more of copper nitrate, copper chloride, copper sulfate, aluminum nitrate, aluminum sulfate, aluminum chloride, ferric nitrate, ferric sulfate, ferric chloride, zinc nitrate, zinc chloride, zinc sulfate, nickel nitrate, nickel sulfate, and nickel chloride.
7. The polishing liquid according to claim 1, characterized in that: The pH regulator is one or more of potassium hydroxide and nitric acid; The silicon carbide polishing liquid also includes 0.01-0.1% of a dispersant; The dispersant includes one or more of polyhydroxy organic matter, ketone organic matter, and ether organic matter; The polyhydroxy organic matter includes one or more of glycerol, cellulose, glucose, sucrose, fructose, ethylene glycol, and starch; the ketone organic matter includes one or more of aliphatic ketones, alicyclic ketones, aromatic ketones, saturated ketones, and unsaturated ketones; the ether organic matter includes RO-R', wherein R is a saturated fatty chain; and R' is a saturated fatty chain.
8. The polishing liquid according to claim 1, characterized in that: The silicon carbide polishing liquid also includes 0.01-5% of a catalyst; the catalyst includes HgCl2, KI, Fe 2+ , rhodium monophosphine water-soluble catalyst, rhodium diphosphine water-soluble catalyst, hydrazine hydrate, triphenylphosphine trissulfonic acid sodium salt, rhodium chloride, p-toluenesulfonic acid, water-soluble organic molybdenum salt, pyridine or imidazole ionic liquid, dichlorodi(1,10-phenanthroline), ammonium molybdate, Cu-polyamide amine complex, Mn-polyamide amine complex, sodium metavanadate, sodium vanadate, InVO4, Cr(VI) or more thereof.
9. A method for preparing the polishing liquid according to any one of claims 1 to 8, comprising: The components are weighed according to weight percentage, the superhard abrasive and the organic abrasive are mixed, and then mixed with other components except the pH adjuster, and then the pH value is adjusted with the pH adjuster to obtain the silicon carbide polishing liquid.
10. A polishing method using the polishing liquid according to any one of claims 1-8, comprising: sticking a silicon carbide material to a polishing head, and polishing the silicon carbide material using the polishing liquid according to any one of claims 1-8.
11. The polishing method according to claim 10, characterized in that: The silicon carbide material is one or more of an insulating silicon carbide wafer, a doped silicon carbide wafer, and a silicon carbide film; the polishing process parameters include: polishing pressure of 3-6psi; polishing pad rotation speed of 50-110rpm; polishing sheet rotation speed of 50-110rpm; polishing liquid flow rate of 30-130mL / min for circulation; and polishing time of 15min-3h.
Citation Information
Cited By
Polishing solution for diamond as well as preparation method and application of polishing solution
CN119875517A
Polishing solution for polishing silicon carbide wafer and preparation method thereof
CN120888243A
A polishing liquid for polishing a silicon carbide wafer and a method for preparing the same
CN120888243B