Multi-element composite magnesium alloy with excellent die-casting manufacturability

By adding Sn elements to magnesium-Al alloy and optimizing element ratio, the high cost and poor processability of magnesium alloys when meeting FAA flame retardant requirements are solved, and the flame retardant performance and casting process performance of magnesium alloys are improved. Meet FAA regulatory requirements and reduce costs.

CN118996219APending Publication Date: 2024-11-22GUANGDONG HUITIAN AEROSPACE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411132140.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When existing magnesium alloy materials meet the FAA flame retardant requirements, there are problems such as high cost, difficult process and poor casting performance. Especially the high cost and poor processability caused by high content of rare earth elements, making it difficult to achieve industrial application.

Method used

By adding carbon group element Sn to the magnesium-Al alloy system and controlling the proportion of multiple elements, reducing the amount of high-cost elements, improving the flame retardant effect and casting process performance of magnesium alloys, Mg-Al-RE-AE- Sn's alloy system optimizes component combinations to achieve efficient continuous production.

Benefits of technology

It significantly improves the flame retardant performance, thermal crack resistance and fluidity of magnesium alloys, reduces costs, improves casting processability, meets the requirements of FAA flame retardant regulations, and is suitable for die-casting and other processes, realizing the industrial application of magnesium alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996219A_ABST
    Figure CN118996219A_ABST
Patent Text Reader

Abstract

The invention provides a magnesium base alloy which comprises the following components in percentage by mass: 5.54%-7.58% of Al, 1.95%-3.51% of RE1, 0%-0.31% of RE2, 1.79%-3.31% of Ca, 0.1%-0.61% of Mn, 0%-0.21% of Zn, 0.11%-1.13% of Sn, RE1 is at least one of La and Ce, RE2 is at least one of Y and Gd, and the balance is magnesium and inevitable impurities.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of nonferrous metal materials, and provides a multi-element composite magnesium alloy material, which has excellent casting performance, complies with FAA\EASA\CCAR flame retardant regulations and meets the lightweight strength requirements of parts. Background Art

[0002] Most of the commercial magnesium alloys that can meet the FAA flame retardant requirements are only WE43 and EV31, both of which are Mg-RE-Zr alloys. Although this alloy system has excellent mechanical strength and flame retardant properties, it has two defects: 1. The precipitation strengthening mechanism of this type of alloy leads to low plasticity of the material, and requires heat treatment, poor casting processability, and is not suitable for high-efficiency die-casting processes and other processing methods that require high processability; 2. In order to meet the flame retardant requirements, high contents of Gd, Y, and Nd elements need to be added to the alloy, which results in high alloy costs and difficult preparation processes.

[0003] In order to solve the above problems, a possible idea is to reduce the content of rare earth elements in the low-cost Mg-Al alloy system and add alkaline earth elements such as Ca to improve the flame retardant properties of magnesium alloys to achieve a balance between cost and performance. However, the difficulty of this idea is that in order to meet the FAA flame retardant requirements, the proportion of each alloy content needs to be accurately controlled to achieve a balance between mechanical properties and cost and processability. In other words, if the amount of elements that can improve the flame retardant effect is too low, there will be no significant improvement effect; and if the amount of such alloying elements is too high, the cost of the alloy will increase, and the casting process properties and mechanical properties such as resistance to thermal cracking and fluidity will be seriously reduced, making it difficult to achieve industrial application. In particular, the addition of Ca in the alkaline earth elements will significantly increase the tendency of the alloy to stick to the mold and thermal cracking, resulting in poor products and high scrap rates during die casting production. Summary of the invention

[0004] In this context, the present invention proposes to reasonably select alloying elements and adjust the proportion of each element, reduce the amount of high-cost elements, enhance the flame retardant effect of magnesium alloy, and improve its casting process performance such as heat cracking resistance and fluidity. According to one aspect of the present invention, by adding the carbon group element Sn to the rare earth-alkaline earth magnesium alloy system and controlling the proportion of multiple elements, the die-casting process of the magnesium alloy is significantly improved without reducing the flame retardant and mechanical properties, thereby achieving efficient continuous production.

[0005] According to one aspect of the present invention, a magnesium-based alloy is provided, characterized in that, in terms of mass percentage, it comprises the following components: Al: 5.54%-7.58%, RE1: 1.95%-3.51%, RE2: 0%-0.31%, Ca: 1.79-3.31%, Mn: 0.1-0.61%, Zn: 0-0.21%, Sn: 0.11-1.13%, wherein RE1 is at least one of La and Ce, RE2 is at least one of Y and Gd, and the rest are magnesium and unavoidable impurities.

[0006] In one embodiment, the Al content ranges from 5.95% to 7.03%, the RE1 content ranges from 2.51% to 3.11%, the RE2 content ranges from 0% to 0.1%, the Ca content ranges from 2.41% to 3.31%, the Sn content ranges from 0.33% to 0.82%, and the Mn content ranges from 0.21% to 0.61%.

[0007] In one embodiment, the content ratio of (La+Ce+Sn) / (Ca) is between 0.66-2.52.

[0008] In one embodiment, the content ratio of (Al) / (Ca+Y+Gd) is between 1.91-3.51.

[0009] According to another aspect of the present invention, a method for preparing a magnesium-based alloy is also proposed, comprising the following steps:

[0010] S1. According to the mass percentage, Mg ingots, Al ingots, Mg-RE1 alloy, Mg-RE2 alloy, Mg-Ca alloy or pure Ca or CaO powder, Sn particles or strips, Mg-Mn alloy or manganese chloride powder are prepared;

[0011] S2. Under a protective atmosphere, the Mg ingot and the Al ingot are melted, the temperature is raised to 700-730° C., the Mg-RE1 alloy, the Mg-RE2 alloy, the Mg-Ca alloy or pure Ca or CaO powder, the Sn particles or strips, the Mg-Mn alloy or the manganese chloride powder are added in sequence, and the mixture is stirred evenly after melting to obtain an alloy melt;

[0012] S3, after standing for 20-35 minutes, degas and add flux, and refine at 700-710℃ for 20-35 minutes;

[0013] S4. After the refining is completed, the mixture is allowed to stand for 0.5-1.0 hours, slag is removed, and casting is performed to obtain the magnesium-based alloy ingot.

[0014] S5, placing the magnesium alloy ingot into a smelting furnace of a die-casting machine for remelting at a smelting temperature of 650-710° C., keeping the ingot at the temperature for more than 20 minutes, and then performing die-casting to obtain a magnesium alloy casting.

[0015] In one embodiment, in step S1, Zn ingots are further configured according to the mass percentage, and in step S2, Zn ingots are first added when the temperature is raised to 700-730°C.

[0016] The present invention also proposes a use of the magnesium-based alloy in the field of aircraft.

[0017] The present invention solves the technical difficulty of balancing the mechanical properties, flame retardant properties and casting process performance of magnesium alloys by adopting composite alloying of carbon group elements, rare earth elements and alkaline earth elements, and effectively improves the castability of the material by constructing an alloy system of Mg-Al-RE-AE-Sn with optimized components. The material is suitable for casting preparation processes such as die casting, but is not limited to this process. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Typical features of the castings used for hot cracking resistance testing are shown and annotated.

[0019] Figure 2 A typical situation for a snake flow test is shown.

[0020] Figure 3 The DSC curve phase diagram of the alloy of the present invention is shown.

[0021] Figure 4 The graph shows the variation of the alloy solid phase ratio with temperature in the embodiment of the present invention. DETAILED DESCRIPTION

[0022] The present invention is described in detail with reference to specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several changes and improvements can be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0023] The preparation methods of each embodiment are as follows:

[0024] S1. According to the mass percentage disclosed in the present invention, Mg ingots, Al ingots, Zn ingots, Mg-RE1 alloy, Mg-RE2 alloy, Mg-Ca alloy or pure Ca or CaO powder, Sn particles or strips, Mg-Mn alloy or manganese chloride powder are prepared;

[0025] S2. Under a protective atmosphere, the Mg ingot and the Al ingot are melted, the temperature is raised to 700-730° C., the Zn ingot, the Mg-RE1 alloy, the Mg-RE2 alloy, the Mg-Ca alloy or pure Ca or CaO powder, the Mg-Mn alloy or manganese chloride powder, the Sn particles or strips are added in sequence, and the mixture is fully stirred after melting to obtain an alloy melt;

[0026] S3, after standing for 20-35 minutes, degas and add flux, and refine at 700-710℃ for 20-35 minutes;

[0027] S4. After the refining is completed, the mixture is allowed to stand for 0.5-1.0 hours, slag is removed, and casting is performed to obtain the magnesium-based alloy ingot.

[0028] S5, placing the magnesium alloy ingot into a smelting furnace of a die-casting machine for remelting at a smelting temperature of 650-710° C., keeping the ingot at the temperature for more than 20 minutes, and then performing die-casting to obtain a magnesium alloy casting.

[0029] The composition of the alloys in various embodiments is shown in Table 1.

[0030] Table 1 Alloy element composition of each example (wt%)

[0031]

[0032]

[0033] When the magnesium alloys of various embodiments are actually prepared, due to the existence of errors, it is impossible to prepare the proportions of various elements completely according to the theoretical values. Therefore, when setting the control group, the invariants of various embodiments in Table 1 fluctuate within the range of ±0.02. This also applies to the values ​​of various comparative examples in Table 3.

[0034] In order to evaluate the performance of the alloy material of the present invention, various tests were performed on the alloys of Examples 1-33, namely: tensile strength test (GB / T228.1 Metal Material Room Temperature Tensile Test Method), flame retardant performance test DOT / FAA / AR / 00 / 12-Chapter 25 (abbreviated as FAA-CH 25), and DOT / FAA / AR / 00 / 12-Chapter 26 (abbreviated as FAA-CH 26). In addition, the present invention also uses a special die-casting mold for testing to compare the thermal cracking resistance and fluidity of each alloy material.

[0035] The FAA Fire Protection Manual Chapter 25 test (DOT / FAA / AR / 00 / 12-Chapter 25, abbreviated as FAA-CH25 in this application) uses a high-intensity, open flame generated by fuel combustion to test the flammability and combustion performance of magnesium alloys used in aviation seat structures to determine whether the alloy can withstand the fire generated after an aircraft crash. Test method: Place a magnesium alloy sample with a thickness of 6.4×width of 38.1×length of 508mm in the flame of an aviation fuel sonic burner (flame temperature requirement: 927℃±55℃) for 4 minutes. The criterion for passing the test is: the sample does not catch fire within the first 2 minutes from being placed in the flame; the weight loss of each sample after the total 4-minute test is completed shall not exceed 10%. The above harsh test conditions mean that the ignition point of the material passing the test must be at least 927℃+55℃=982℃, and even if it is ignited after 2 minutes due to the increase in cumulative heat, it cannot continue to burn thereafter (otherwise the weight loss will be significantly more than 10%). This requires the magnesium alloy material to have a high ignition point and good self-extinguishing properties.

[0036] The FAA Fire Protection Manual Chapter 26 test (DOT / FAA / AR / 00 / 12-Chapter26, abbreviated as FAA-CH26 in this application) uses an electric heat radiation plate and a propane jet flame to test the flammability and combustion performance of aircraft cabin magnesium alloy structural components to determine whether the material can self-extinguish in time when a cabin fire occurs during flight. The sample size is 152.4mm long × 76.2mm wide × 0.64mm thick. The specific method is: put the sample into a closed test box containing an electric radiation plate and a propane igniter, spray the propane flame onto the surface of the sample, keep it for 2 minutes, then move the propane flame away, and continue to observe for 2 minutes. During the test, the temperature of the electric radiation plate is set to 232±55℃, and the propane flame is about 127 mm long. The criterion for passing the test is: the sample is ignited at least 30 seconds after contacting the flame of the igniter; the weight loss of the sample after the test is completed shall not exceed 30%. According to public information, the maximum temperature of the propane flame can reach about 2000℃. Compared with the test method in Chapter 25 of the FAA Fire Protection Manual, although the ignition time requirements and specimen weight loss requirements of FAA-CH26 are relaxed, due to the high temperature of the propane flame itself and the thinner specimen (thinner combustibles are more flammable), the FAA Fire Protection Manual Chapter 26 test still places high requirements on the ignition point and self-extinguishing ability of magnesium alloys.

[0037] See also Figure 1 The test method for thermal crack resistance is to use a special mold to die-cast the parts, for example, mark 30 typical die-casting structural features, and count the number of thermal cracks in the above typical structural features. The statistical formula for thermal crack resistance is as follows. The higher the percentage of thermal crack resistance, the worse the thermal crack resistance, and vice versa.

[0038]

[0039] See also Figure 2 The fluidity test method is to use a serpentine die-casting mold to measure the fluidity of the alloy based on its flow length. The longer the length, the better the fluidity of the alloy.

[0040] The test results of each test are shown in Table 2.

[0041] Table 2 Mechanical and flame retardant properties, thermal crack resistance, and fluidity test results of each embodiment

[0042]

[0043]

[0044] The Mg-Al-RE-AE system used in the present invention can effectively take into account flame retardancy, mechanical properties, and casting process performance. The main functions of each element are as follows:

[0045] Al is a commonly used strengthening element for magnesium alloys. It can not only effectively ensure the strength of magnesium alloys, but also improve the casting process performance of magnesium alloys. When the aluminum content is low, the strength of the alloy is improved less and the casting performance is also poor; when the aluminum content is too high, it will have an adverse effect on the flame retardant properties. Therefore, the range of aluminum used in this alloy is exemplarily between 5.54-7.58%.

[0046] Rare earth elements La or Ce in magnesium-aluminum alloys can effectively change the quantity, morphology and distribution of Mg-Al phases in Mg-Al alloys by forming high melting point Al-La / Ce alloy phases, and can significantly improve the room temperature and high temperature mechanical properties of the alloys. Due to the high temperature stability of the Al-La / Ce phase, the high temperature oxidation of the magnesium matrix is ​​slowed down, and the flame retardant properties of the alloys are improved. The range of La or Ce elements is exemplarily between 1.95-3.51%.

[0047] Heavy rare earth elements Y and Gd do not form sharp rod-like phases in magnesium, and can be well dissolved in the magnesium matrix, promoting the precipitation of light rare earth elements and increasing the nucleation density of the alloy. Therefore, the composite application with light rare earth elements has a better multi-element microalloying strengthening effect, which can improve the mechanical properties of magnesium alloys and obtain better strength and toughness. At the same time, Y and Gd also have a positive effect on the rapid self-extinguishing tendency of magnesium alloys. The range of Y or Gd elements is exemplarily between 0-0.31%.

[0048] The Mn element can prevent the recrystallization process of aluminum alloys, increase the recrystallization temperature, and significantly refine the recrystallized grains. The refinement of the recrystallized grains is mainly through the Al-Mn compound dispersed particles that hinder the growth of recrystallized grains. Another function of Mn is to dissolve impurity iron (Fe) and reduce the harmful effects of iron. The Mn element content is exemplarily 0.1-0.61%.

[0049] The Ca element can inhibit the high-temperature oxidation of magnesium alloys, increase the ignition point of magnesium alloys, and promote the refinement of magnesium alloy grains during the solidification process. In a high-temperature molten state, the calcium element diffuses preferentially to the liquid surface, combines with oxygen before the magnesium element, and forms a dense oxide film, which hinders the further oxidation of the magnesium element, thereby improving the high-temperature performance of the magnesium alloy. However, excessive calcium content will lead to poor thermal cracking resistance of magnesium alloy castings and significantly reduce the mechanical properties of the alloy. In this application, the range of the Ca element is illustratively 1.79-3.31%.

[0050] Sn element exists in magnesium alloy mainly in the form of high temperature stable alloy phases such as Mg2Sn or CaMgSn, which is beneficial to the high temperature performance and thermal stability of the alloy. The present invention also unexpectedly noticed that adding a small amount of Sn element can effectively improve the casting performance of the Mg-Al-RE-AE alloy system. With the increase of Sn content, the fluidity, thermal cracking resistance and anti-sticking performance of the alloy are improved, but too much Sn is not conducive to casting performance.

[0051] The present invention also unexpectedly discovered that the (La+Ce+Sn) / Ca content ratio R1 and the Al / (Ca+Y+Gd) content ratio R2 in the alloy applied for by the present invention have a unique effect on coordinating mechanical properties, flame retardant properties, and casting process performance.

[0052] It can be seen from Tables 1 and 2 that the alloy of the present invention has good mechanical properties and flame retardant properties, and has casting fluidity and thermal cracking resistance comparable to that of the AZ91 alloy (ie, Comparative Example 1 in Table 3).

[0053] Specifically, it can be seen from Examples 1-5 that as the total amount of aluminum elements increases, the mechanical strength of the alloy gradually increases, the plasticity slightly decreases, the thermal cracking resistance and fluidity are significantly improved, but the flame retardant performance measured by the weight loss rate of the CH26 flame retardant test decreases significantly, indicating that a low melting point phase containing aluminum appears, which reduces the ignition temperature of the alloy.

[0054] It can be seen from Examples 1 and 6-9 that La has an effect on the mechanical, flame retardant and casting properties of the alloy. The alloy strength first increases and then decreases with the increase of La, while the alloy plasticity decreases with the increase of rare earth content. The inventors believe that this is because the main strengthening phase Al 11As La3 / Al2La increases, the alloy strength increases with the amount of strengthening phase, but due to Al 11 The La3 / Al2La phase will grow rapidly with the increase of the total amount of rare earth, resulting in the coarsening of the alloy microstructure, thereby reducing the alloy plasticity.

[0055] It can be seen from Examples 1, 10, and 11 that the flame retardant properties are particularly sensitive to the Ca content. When the Ca content is about 2%, the weight loss rate is 28%, which is close to the threshold required by CH26 (less than 30%). As the Ca content increases, the flame retardant properties gradually improve, and even no combustion occurs. However, the increase in Ca content will increase the brittleness of the alloy, resulting in a decrease in both strength and elongation. As the Ca content increases, the thermal cracking resistance and flow properties decrease.

[0056] From the comparison between Example 1 and Examples 16-19, it can be seen that the thermal cracking resistance and casting performance of the alloy can be significantly improved with the increase of Sn element, the strength first increases and then decreases, and the plasticity first decreases and then increases.

[0057] It can be seen from Example 1 and Examples 20-21 that adding Zn element can improve the strength and casting fluidity of the alloy, but as the Zn element content increases, the plasticity, flame retardancy and thermal cracking resistance of the alloy of the present invention will deteriorate with the increase of Zn element.

[0058] It can be seen from Example 1 and Examples 22-23 that the Mn element can improve the yield strength, fluidity and thermal cracking resistance of the alloy.

[0059] It can be seen from Example 1 and Examples 24-25 that with the increase of the Y and Gd element contents, the strength and plasticity have no obvious changes, but the flame retardant properties have an optimization trend, the fluidity has a decreasing trend, and the thermal cracking tendency has an increasing trend.

[0060] It can be seen from Example 1 and Examples 12-15 that the content ratio R1 of (La+Ce+Sn) / Ca and the content ratio R2 of Al / (Ca+Y+Gd) have a significant effect on the mechanical properties, flame retardancy, casting heat cracking resistance and fluidity of the alloy of the present invention. When the above ratios are high, the flame retardancy is poor, and the casting fluidity and heat cracking resistance are significantly improved. On the contrary, when the above ratios R1 and R2 are low, the flame retardancy is significantly improved, and the casting fluidity and heat cracking resistance are poor.

[0061] It can be seen from Example 1 and Examples 26-29 that the Ce element can effectively replace the La element. The alloy strength first increases and then decreases with the increase of the Ce element, and the alloy plasticity decreases with the increase of the rare earth content. This is because the main strengthening phase of the alloy, the Al-Ce phase, has similar properties to the Al-La phase. The increased Al-Ce phase leads to increased alloy strength, but the Al-Ce phase grows rapidly with the increase of the total amount of rare earths, resulting in coarsening of the alloy microstructure, thereby reducing the alloy plasticity.

[0062] It can be seen from Example 1 and Examples 30-33 that, when the total amount of La and Ce remains unchanged, the alloy properties obtained with different ratios of La and Ce are equivalent, and the change in the ratio between the two has little effect on the various properties.

[0063] In order to further evaluate the various properties of the magnesium alloy of the present invention, comparative examples were designed and prepared, wherein comparative example 1 is a standard process scheme for an industrial general grade AZ91 magnesium alloy, and comparative examples 2-19 are designed as process schemes for comparison with the embodiments of the present invention. The elemental compositions of each comparative example are shown in Table 3.

[0064] Table 3 Alloy element composition of each comparative example (wt%)

[0065]

[0066]

[0067] The alloys for the comparative examples were subjected to tensile strength test (GB / T228.1 Metal Material Room Temperature Tensile Test Method), flame retardant test (DOT / FAA / AR / 00 / 12-Chapter 25, DOT / FAA / AR / 00 / 12-Chapter 26), casting fluidity and thermal cracking resistance test. The test results are shown in Table 4.

[0068] Table 4 Mechanical and flame retardant properties, thermal crack resistance, and fluidity test results of each comparative example

[0069]

[0070] It can be seen from the test results in Table 4 that, compared with the AZ91 magnesium alloy (Comparative Example 1), the alloy of the present invention has outstanding flame retardant properties and comparable casting properties and mechanical properties.

[0071] It can be seen from Example 1 and Comparative Examples 2-3 that too high an Al element will lead to a sharp decrease in the flame retardancy, while too low an Al element will cause the die-casting fluidity and thermal cracking resistance of the alloy to deteriorate seriously.

[0072] It can be seen from Example 1 and Comparative Examples 4-5 that when the La content reaches a certain value, the strength of the alloy no longer increases, but it also does not decrease significantly. When the La content is low, the strength of the alloy decreases significantly.

[0073] It can be seen from Example 1 and Comparative Examples 6-7 that too much Ca content will lead to serious deterioration of mechanical properties, die-casting fluidity and thermal cracking resistance, and when the Ca content is too low, the flame retardant properties will drop sharply.

[0074] It can be seen from Example 1, Comparative Examples 2-3, 6-7, 8-9 that if the mass ratio R1 of (La+Ce+Sn) / (Ca) and the mass ratio R2 of Al / (Ca+Y+Gd) are too high, the flame retardant performance cannot meet the requirements of FAA regulations. If the ratios R1 and R2 are too low, the casting performance deteriorates seriously.

[0075] It can be seen from Example 1 and Comparative Examples 10-11 that when the Sn element is high, although the casting fluidity is improved, the strength and hot cracking performance are greatly reduced. When Sn is not added, the casting fluidity and hot cracking resistance are significantly reduced.

[0076] It can be seen from Example 1 and Comparative Example 12 that when Zn is too high, the strength is improved, but the thermal cracking resistance is seriously deteriorated.

[0077] It can be seen from Example 1 and Comparative Examples 13-14 that as the Mn content decreases, the strength of the alloy decreases, and the casting fluidity and thermal cracking resistance also decrease.

[0078] It can be seen from Example 1 and Comparative Example 15 that excessive addition of Y and Gd elements will lead to decreased casting fluidity and thermal cracking resistance.

[0079] It can be seen from Examples 26-29 and Comparative Examples 16-17 that when the Ce content reaches a certain value, the strength of the alloy no longer increases, but it also does not decrease significantly. When the Ce content is low, the strength of the alloy decreases significantly.

[0080] By comparing Examples 1 and 30-33 and Comparative Examples 18-19, when the total content of La+Ce elements exceeds a certain value, the strength of the alloy no longer increases significantly, the plasticity decreases, the flame retardancy remains excellent, the fluidity increases slightly, and the thermal cracking tendency is poor; when the total content of La+Ce elements is low, the strength of the alloy decreases significantly, the plasticity improves, but the flame retardancy decreases, the fluidity deteriorates, and the thermal cracking tendency is also poor.

[0081] Next, the theoretical relationship between the element content in magnesium alloy and the properties of magnesium alloy is explained.

[0082] 1. Flame retardant properties

[0083] Both the test methods of Chapter 25 of the FAA Fire Prevention Manual and the test of Chapter 26 of the FAA Fire Prevention Manual put forward the dual requirements of high ignition point + high self-extinguishing ability for the flame retardant mode of magnesium alloys, and the above two requirements mean that it is necessary to control the chemical and physical properties of the magnesium alloy before combustion and the properties of the magnesium alloy after combustion at the same time. In the prior art, in order to achieve the flame retardant effect of magnesium alloys, the commonly used method is to adjust the ratio of chemical elements in the magnesium alloy to form different high melting point phases so as to increase the ignition point of the magnesium alloy; however, there is no description of the self-extinguishing ability and phenomenon of the magnesium alloy after it has started to burn. On the contrary, in the present invention, while increasing the ignition point of the magnesium alloy, by controlling the content and ratio of rare earth and alkaline earth elements in the magnesium alloy, a combustion product containing Ca and rare earth elements is obtained after the magnesium alloy is burned. The rapid aggregation of the combustion products on the surface of the magnesium alloy isolates the air so as to hinder the oxidation reaction (combustion process) of the magnesium alloy and achieve the purpose of rapid self-extinguishing.

[0084] The basic principle of magnesium alloy combustion is that magnesium vapor and oxygen undergo a violent oxidation reaction under high temperature. 17 Al 12 The melting point is low and mainly distributed at the grain boundaries. In a high temperature environment, it is very easy to melt, causing the magnesium vapor inside the magnesium matrix to quickly diffuse to the surface along the damaged grain boundaries, causing the magnesium vapor partial pressure on the surface to increase rapidly, and finally violent oxidation reaction (combustion) occurs after contact with air. Therefore, controlling the contact process between magnesium vapor and air is the key to controlling the ignition time and self-extinguishing time of magnesium alloy.

[0085] The present invention adds light rare earth La and alkaline earth Ca in combination to make the Mg in the eutectic region 17 Al 12 phase disappears and is replaced by Al 11 The high melting point alloy phase mainly composed of La3 and (MgAl)2Ca, etc., reduces the generation of magnesium vapor inside the magnesium alloy, slows down the partial pressure of magnesium vapor on the surface, and thus greatly improves the ignition point of the magnesium alloy. From the DSC test results made by the inventor ( Figure 3 ) shows that in the temperature range of 400-490℃, the curve is smooth and there is no heat change peak caused by solid phase transition (Mg 17 Al 12 The eutectic temperature of the alloy phase is 437°C. This indicates that Mg 17 Al 12 The alloy phase has disappeared from the alloy material of the present invention.

[0086] In addition, when the magnesium alloy to which La and Ca are added in this case burns, due to the surface activity of La and Ca, they will preferentially segregate and aggregate on the surface of the magnesium alloy, reducing the partial pressure of magnesium vapor on the surface of the magnesium alloy, and La and Ca will preferentially react with oxygen to generate oxides located on the surface of the magnesium alloy, reducing the contact between magnesium vapor and air. Unlike the loose and porous MgO film, the La2O3 film and the CaO / MgO composite film are more continuous and dense. They are located on the outermost layer of the burning magnesium alloy, greatly reducing the contact between oxygen in the air and magnesium, making the burning magnesium alloy self-extinguish faster. Different rare earth / alkaline earth contents and ratios affect the formation effect of the continuous and dense oxide film, thereby affecting the self-extinguishing time of the magnesium alloy.

[0087] Although magnesium alloys with elements such as La or Ca are mentioned in the prior art, the inventors of the present invention realized based on a large number of experiments that good flame retardant and self-extinguishing effects cannot be obtained by randomly adding La and Ca (as well as Y or Gd). The inventors believe that when La and Ca are too little, the high-melting-point alloy phase cannot sufficiently replace the low-melting-point phase inside the magnesium-aluminum alloy, causing the internal magnesium vapor to still diffuse outward, making the magnesium alloy still flammable; and when La and Ca (as well as Y or Gd) are too little or the ratio is not appropriate, the amount and continuous density of the oxide film formed are not enough to prevent the magnesium vapor from contacting with oxygen, and the magnesium alloy cannot be made to self-extinguish quickly. When there is too much La, more Al2O3 will be generated in the tissue. 11 La3, distributed in grain boundaries and grains, will seriously affect the uniformity of La in the magnesium matrix, affect the consistency and uniformity of the oxide film, and ultimately lead to a loose and porous oxide layer, resulting in poor self-extinguishing effect. When the Ca content is too high, it will deteriorate the casting process performance and mechanical properties of the alloy.

[0088] Therefore, the inventors realized that it is necessary to determine the specific ratio and range of each element in the magnesium alloy and achieve a reasonable combination of the content of each element, so as to simultaneously meet the requirements of both ignition time and self-extinguishing time, and ensure the processing performance and mechanical properties of the magnesium alloy.

[0089] The alloy material applied for in this case will not burn in the test of Chapter 25 of the FAA Fire Manual, and the weight loss rate is 0%. In the test of Chapter 26 of the FAA Fire Manual, some alloy materials with certain proportions will not burn, and some alloy materials with certain proportions will burn and quickly extinguish themselves after the fire source is removed. The above two tests meet the requirements of magnesium alloy fire retardancy.

[0090] 2. Casting performance

[0091] 2.1 Analysis of thermal cracking resistance of the alloy of the present invention

[0092] From the molten state to the completely solid state, as the temperature drops, the solidification of the metal can usually be divided into four stages: the liquid phase free feeding stage, the large-scale feeding stage between crystals, the small-scale feeding stage between crystals, and the complete solidification stage between crystals.

[0093] In the liquid phase free shrinkage stage, the metal is completely in a molten state, the metal liquid can flow freely and no solidification shrinkage force is generated, so there will be no thermal crack initiation;

[0094] During the large-scale feeding stage between crystals, solid phase begins to precipitate in the melt and a small amount of dendrites begin to overlap, but most of the liquid phase can still flow between dendrites. Therefore, if dendrite separation and disconnection occur, the residual liquid phase can also be quickly fed to avoid the initiation and expansion of thermal cracks.

[0095] In the stage of small-scale intergranular shrinkage feeding, the dendrites are basically overlapped and form a skeleton. Only a small amount of liquid phase remains in the melt and its flow is hindered by the developed dendrite network, which significantly reduces the liquid phase's ability to heal cracks. At the same time, the alloy solidification shrinkage is large at this stage. If the dendrite skeleton strength and intergranular bonding force cannot withstand the solidification shrinkage force at this time, thermal cracks will initiate and cannot be promptly fed by the residual liquid phase, which can easily cause thermal cracking defects in the casting.

[0096] In addition, during the solidification process, the range from the temperature at which the dendrites begin to contact to the solidus temperature of the alloy is generally called the brittle temperature range. In this temperature range, the alloy has very low plasticity and is prone to thermal cracking. The larger the solidification range of the alloy, the larger its brittle temperature range. The smaller the proportion of the brittle temperature range in the solidification process or the higher the alloy strength, the lower the alloy's thermal cracking sensitivity.

[0097] The material factors that affect the hot cracking tendency of alloys include the solidification temperature range, the type and evolution of the second phase, the content and morphological distribution of the eutectic structure, and the grain size.

[0098] In the present invention, by comparing the solid phase ratio of Examples 10 and 11 and Example 1 with the change of temperature, the solidification temperature range of the alloy can be effectively adjusted by adding Sn element and strictly controlling the range of the content ratio R1 of (La+Ce+Sn) / Ca and the content ratio R2 of Al / (Ca+Y+Gd). Figure 4 ). With the increase of Sn content and R1 value, the temperature range of the solid-liquid two-phase region first decreases and then increases, and the brittle temperature range of the two-phase region also first decreases and then increases. (Comparative Example 11#, Example 1# and Comparative Example 10#).

[0099] In addition, the alloy system of the present invention mainly includes second phases such as (Mg, Al)2Ca, Mg2Ca, Mg2Sn, CaMgSn, Al2Ca, Al-RE, etc. By adjusting the content ratio R1 of (La+Ce+Sn) / Ca and the content ratio R2 of Al / (Ca+Y+Gd) in the alloy, the amount and morphological distribution of the second phase in the alloy can be adjusted during the solidification process of the alloy of the present invention.

[0100] The content ratio R1 of (La+Ce+Sn) / Ca mainly describes the relationship between Sn, Ca and rare earth. During the solidification process, the CaMgSn phase that precipitates first will inhibit the formation of the Mg2Sn phase and Mg2Ca phase that precipitate later. The first precipitated phase will form the core of heterogeneous nucleation, resulting in grain refinement and the effect of reducing the spacing between secondary dendrite arms, while blocking the generation of continuous coarse Al-RE phase, making the other second phases of the alloy more refined. The inventors realized that grain refinement can improve the thermal cracking resistance of the alloy. This is because under the same strain, the coarsening of the grains reduces the number of liquid films between the grains in the late solidification period, and a single liquid film will be subjected to a large strain, and thermal cracks are easy to initiate.

[0101] 2.2 Fluidity analysis of the alloy of the present invention

[0102] The ability of liquid alloy to fill the mold cavity and make the casting shape complete and clear is called the filling capacity of the alloy. Fluidity is a quantifiable indicator of alloy filling capacity and can be used as one of the evaluation indicators of casting performance. The material factors that affect the fluidity of the alloy mainly include the solidification temperature range of the alloy, the second phase, the viscosity of the alloy, etc.

[0103] The change in the solid-liquid two-phase range during the alloy solidification process will affect the fluidity of the alloy. When the solid-liquid two-phase region increases, the dendrites are generally more developed and tend to solidify in a paste state, which is not conducive to improving the fluidity of the alloy. As shown above, in the alloy of the present invention, by adding the Sn element and strictly controlling the range of the (La+Ce+Sn) / Ca content ratio R1 and the Al / (Ca+Y+Gd) content ratio R2, the solidification temperature range of the alloy can be effectively adjusted. With the increase of Sn content and R1 value, the temperature range of the solid-liquid two-phase region first shrinks and then increases. Reasonable Sn content and R1, R2 ratios can obtain a smaller solid-liquid two-phase region, which is beneficial to improving the fluidity of the alloy.

[0104] In addition, the change of the precipitated phase or the primary phase during the solidification process of the alloy will also affect the fluidity of the alloy. During the solidification process of the alloy of the present invention, at a relatively high temperature, the Sn element preferentially precipitates the CaMgSn phase and the Mg2Sn phase, and the Al element preferentially forms the Al2Y phase, the (Mg, Al)2Ca phase, and the Al-RE phase. These high-temperature precipitated phases are formed at the beginning of the solidification of the alloy, and are enriched at the front of the solid-liquid interface, hindering the growth of the grains, causing the second phase to be dispersed, and prolonging the formation time of the network structure, thereby improving the fluidity of the alloy. In the alloy of the present invention, by controlling the range of the content ratio R1 of (La+Ce+Sn) / Ca and the content ratio R2 of Al / (Ca+Y+Gd), the amount and morphology of the precipitated phase and the primary phase can be adjusted, thereby improving the fluidity of the alloy of the present invention.

[0105] The viscosity of the alloy will also affect the fluidity of the alloy. The fluidity of the alloy liquid with high viscosity is poor, and the viscosity of the alloy with low viscosity is also low. The viscosity of the liquid alloy is mainly affected by the inclusion content and its physical properties in the alloy. The increase in the content of solid inclusions will increase the viscosity of the alloy. Since magnesium alloys are easily oxidized, there are many non-metallic oxides such as MgO and Al2O3 in the alloy liquid. The melting points of these oxides are very high, such as the melting point of MgO is 2800℃ and the melting point of Al2O3 is 2055℃. These inclusions appear in the magnesium alloy liquid in a solid state, which increases the viscosity and causes the fluidity of the alloy to decrease. The stronger the antioxidant ability of the alloy melt, the less oxide particles such as MgO will be formed, the less likely the alloy viscosity will increase, and the better the fluidity will be. The rare earth elements Y, La, and Ce added to the alloy of the present invention are all surface active elements, so that a dense rare earth oxide film is preferentially formed on the surface of the molten metal, avoiding the generation of oxides such as MgO, improving the antioxidant ability of the overall melt, cleaning the magnesium alloy melt, reducing the viscosity of the alloy liquid, and improving the fluidity of the alloy.

[0106] In general, based on theoretical analysis and experimental verification, the inventors rationally selected various elements and their proportions, ensuring the flame retardant and mechanical properties of the magnesium alloy while ensuring the thermal cracking resistance and fluidity of the magnesium alloy, thereby improving the casting performance of the magnesium alloy.

[0107] By means of the technical solution of the present invention, many advantages can be achieved, for example:

[0108] (1) Solved the difficulty of magnesium alloys meeting FAA flame retardant regulations;

[0109] (2) Reduce costs. Specifically, the magnesium alloy material of the present invention not only meets the higher requirements of FAA flame retardant regulations, but also uses lower cost elements than existing WE43 and EV31 magnesium alloys. The magnesium alloy material of the present invention is particularly helpful in achieving lightweight aircraft when used in aircraft.

[0110] (3) Significantly improved the die-casting thermal cracking resistance and fluidity of rare earth alkaline earth magnesium alloys.

Claims

1. A magnesium-based alloy, It is characterized in that Calculated by mass percentage, it includes the following components: Al: 5.54%-7.58%, RE1: 1.95%-3.51%, RE2: 0%-0.31%, Ca: 1.79-3.31%, Mn: 0.1-0.61%, Zn: 0-0.21%, Sn: 0.11-1.13%, wherein RE1 is at least one of La and Ce, RE2 is at least one of Y and Gd, and the rest are magnesium and unavoidable impurities.

2. A magnesium-based alloy according to claim 1, It is characterized in that The Al content ranges from 5.95% to 7.03%, the RE1 content ranges from 2.51% to 3.11%, the RE2 content ranges from 0% to 0.1%, the Ca content ranges from 2.41% to 3.31%, the Sn content ranges from 0.33% to 0.82%, and the Mn content ranges from 0.21% to 0.61%.

3. The magnesium-based alloy according to claim 1 or 2, It is characterized in that The ratio of (La+Ce+Sn) / (Ca) content is between 0.66-2.

52.

4. The magnesium-based alloy according to claim 1 or 2, It is characterized in that The (Al) / (Ca+Y+Gd) content ratio is between 1.91-3.

51.

5. A method for preparing a magnesium-based alloy according to any one of claims 1 to 4, It is characterized in that The steps include: S1. According to the mass percentage, Mg ingots, Al ingots, Mg-RE1 alloy, Mg-RE2 alloy, Mg-Ca alloy or pure Ca or CaO powder, Sn particles or strips, Mg-Mn alloy or manganese chloride powder are prepared; S2. Under a protective atmosphere, the Mg ingot and the Al ingot are melted, the temperature is raised to 700-730° C., the Mg-RE1 alloy, the Mg-RE2 alloy, the Mg-Ca alloy or pure Ca or CaO powder, the Sn particles or strips, the Mg-Mn alloy or the manganese chloride powder are added in sequence, and the mixture is stirred evenly after melting to obtain an alloy melt; S3, after standing for 20-35 minutes, degas and add flux, and refine at 700-710℃ for 20-35 minutes; S4. After the refining is completed, the mixture is allowed to stand for 0.5-1.0 hours, slag is removed, and casting is performed to obtain the magnesium-based alloy ingot. S5, placing the magnesium alloy ingot into a smelting furnace of a die-casting machine for remelting at a smelting temperature of 650-710° C., keeping the ingot at the temperature for more than 20 minutes, and then performing die-casting to obtain a magnesium alloy casting.

6. A preparation method according to claim 5, It is characterized in that In step S1, Zn ingots are also configured according to the mass percentage, and in step S2, Zn ingots are first added when the temperature is raised to 700-730°C.

7. Use of the magnesium-based alloy according to any one of claims 1 to 4 in the field of aircraft.