Aluminum etching solution as well as preparation method and application thereof

By adding specific combinations of inorganic acids, organic acids, corrosion inhibitors and leveling agents to the aluminum etching liquid, the problems of uneven etching of aluminum layer thickness and equipment corrosion are solved, and the efficient and uniform aluminum etching process is achieved. .

CN118996422APending Publication Date: 2024-11-22SUZHOU XINGYI NEW MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411104223.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the 3C electronic manufacturing process, when the aluminum layer is thicker, the existing aluminum etching liquid can easily lead to uneven etching and uneven lines when accelerating the etching rate, and the equipment is prone to corrosion.

Method used

Aluminum etching liquid is used, containing inorganic acids, organic acids, corrosion inhibitors (boric acid compounds), leveling agents (compounds containing strong electron-absorbing groups and sulfonic acid groups on the benzene ring), surfactants and wet The agent is prepared evenly by stirring, and is used to improve the etching rate and uniformity and protect the equipment.

Benefits of technology

High etching rate (up to 4μm/min) and uniformity are achieved, corrosion of titanium and other metals on the surface of the equipment is avoided, and the flatness of the aluminum circuit is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996422A_ABST
    Figure CN118996422A_ABST
Patent Text Reader

Abstract

The invention relates to an aluminum etching solution as well as a preparation method and application thereof, and belongs to the technical field of aluminum etching solutions. The aluminum etching liquid comprises the following components in percentage by weight: 5%-20% of inorganic acid, 0.1%-1% of organic acid, 0.1%-2% of a corrosion inhibitor, 0.5%-3% of a leveling agent, 0.1%-1.5% of a surfactant, 1%-10% of a wetting agent and the balance of water. The corrosion inhibitor is selected from boric acid compounds. The aluminum etching solution is high in etching rate, and the highest etching rate can reach about 4 microns / min; the etching is uniform, and the etched circuit is relatively smooth; in the using process, the problem of corrosion of metal such as titanium on the surface of equipment is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum etching liquid, and in particular relates to an aluminum etching liquid and a preparation method and application thereof. Background Art

[0002] There are two common types of aluminum etching solutions: one is acidic etching, such as phosphoric acid system or hydrochloric acid system; the other is a strong alkaline system. This is because aluminum metal is an amphoteric metal, which can react with both acid and alkali. In addition, after aluminum is oxidized, it will form a dense aluminum oxide structure, which has a very stable configuration and is resistant to concentrated sulfuric acid and concentrated nitric acid. It also has a certain corrosion resistance to normal acids and alkalis.

[0003] The aluminum layers in common chip manufacturing and advanced packaging fields are relatively thin, usually not exceeding 1 micron, so the etching solutions used are basically phosphoric acid systems, and nitric acid and acetic acid are usually added to the phosphoric acid system. Nitric acid is oxidizing, which can evenly convert aluminum into aluminum oxide. In this case, phosphoric acid can evenly etch the aluminum oxide layer, so there will be no phosphoric acid and aluminum and aluminum oxide reacting separately, causing uneven etching. Acetic acid has some wettability during the etching process, and can also enhance the uniformity of etching. However, in the 3C electronic manufacturing process (flexible light strips, panel displays, etc.), the aluminum layer may be tens of microns thick, and it usually takes several minutes to etch completely. Etching with a phosphoric acid system is relatively slow. At this time, a hydrochloric acid system may be needed, but at a higher etching rate, uneven etching often occurs, and the lines are uneven. Especially when the rate of the aluminum etching solution is accelerated, this uneven situation is significantly aggravated.

[0004] Therefore, developing an aluminum etching solution with high etching rate, uniform etching and smooth circuit is still a problem that needs to be solved urgently. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides an aluminum etching solution and a preparation method and application thereof.

[0006] The first object of the present invention is to provide an aluminum etching solution, which comprises, by weight, 5%-20% of an inorganic acid, 0.1%-1% of an organic acid, 0.1%-2% of a corrosion inhibitor, 0.5%-3% of a leveling agent, 0.1%-1.5% of a surfactant, 1%-10% of a wetting agent, and the balance is water; the corrosion inhibitor is selected from boric acid compounds.

[0007] In one embodiment of the present invention, the boric acid compound is selected from one or more of boric acid, sodium borate, potassium borate, aluminum borate and zinc borate.

[0008] In one embodiment of the present invention, the inorganic acid is selected from one or more of hydrochloric acid, phosphoric acid, hydrofluoric acid and hydroiodic acid.

[0009] In one embodiment of the present invention, the organic acid is selected from one or more of formic acid, acetic acid, propionic acid, oxalic acid, malonic acid, butyric acid, succinic acid, valeric acid and glutaric acid.

[0010] In one embodiment of the present invention, the leveler is selected from one or more of benzenesulfonic acid, fluorobenzenesulfonic acid, halogenated benzenesulfonic acid, trifluoromethylbenzenesulfonic acid and nitrobenzenesulfonic acid.

[0011] In one embodiment of the present invention, the surfactant is selected from one or more of bisphenol A polyoxyethylene ether, lauryl alcohol polyoxyethylene ether, secondary alcohol polyoxyethylene ether and nonylphenol polyoxyethylene ether.

[0012] In one embodiment of the present invention, the wetting agent is a fatty alcohol compound.

[0013] In one embodiment of the present invention, the fatty alcohol compound is selected from one or more of 1-propanol, 2-propanol, butanol, 1,2-propylene glycol, 1,3-propylene glycol, glycerol, butanediol and pentanediol.

[0014] The second object of the present invention is to provide a method for preparing the aluminum etching solution, characterized in that it comprises the following steps: stirring an inorganic acid, an organic acid, a corrosion inhibitor, a leveling agent, a surfactant, a wetting agent and water to obtain the aluminum etching solution.

[0015] The third object of the present invention is to provide an application of the aluminum etching solution in an electronic manufacturing process, specifically, metal aluminum etching in a flexible light strip and a display panel manufacturing process.

[0016] The technical solution of the present invention has the following advantages over the prior art:

[0017] (1) The leveling agent used in the aluminum etching solution of the present invention is a leveling agent containing strong electron-withdrawing groups and sulfonic acid groups on the benzene ring, which has a very obvious effect on the flatness and uniformity of the aluminum circuit; at the same time, the higher its content, the aluminum etching rate will also increase slightly. The reason for the unevenness of the circuit is that there is an aluminum oxide layer with inconsistent thickness on the surface of the aluminum, and the aluminum oxide layer is more difficult to etch than the aluminum layer. The introduction of this leveling agent containing sulfonic acid groups and the strong electron-withdrawing groups on the benzene ring can enhance the acidity of the sulfonic acid group and promote the etching of aluminum oxide, thereby improving the flatness and uniformity of etching. In addition, in these strong acid environments, many devices are easily corroded. Using boric acid compounds containing boric acid groups as corrosion inhibitors and using the regulation and buffering effect of boric acid on pH value can effectively reduce the corrosion of metals such as titanium on the surface of the equipment due to excessive acidity.

[0018] (2) The aluminum etching solution of the present invention has a high etching rate, which can reach up to about 4 μm / min at most; the etching is uniform, and the circuit after etching is relatively flat; during use, it will not cause corrosion problems of metals such as titanium on the surface of the equipment. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:

[0020] Figure 1 The etching effect of the aluminum etching solution of Example 5 of the present invention;

[0021] Figure 2 This is the etching effect of the aluminum etching solution of Comparative Example 5 of the present invention. DETAILED DESCRIPTION

[0022] When the traditional phosphate aluminum etching solution is used for etching thick aluminum layers in 3C electronic manufacturing processes (flexible light strips, panel displays, etc.), the etching rate is relatively low. If the hydrochloric acid aluminum etching solution is used to speed up the etching speed, the uniformity of aluminum circuit etching will decrease. If you want to improve the uniformity through oxidants, the etching rate may be reduced. At the same time, some additives will damage the upper dry film, green oil and other barrier layers of the aluminum etching circuit, affecting the subsequent processes. If the aluminum etching rate is accelerated, the acidity will increase, which will cause corrosion to equipment or metals such as titanium.

[0023] In order to solve the above technical problems, the present invention provides an aluminum etching solution and a preparation method and application thereof. The aluminum etching solution has a high etching rate and good etching uniformity and does not corrode equipment and other protective metals such as titanium.

[0024] The first object of the present invention is to provide an aluminum etching solution, which comprises, by weight, 5%-20% of an inorganic acid, 0.1%-1% of an organic acid, 0.1%-2% of a corrosion inhibitor, 0.5%-3% of a leveling agent, 0.1%-1.5% of a surfactant, 1%-10% of a wetting agent, and the balance is water; the corrosion inhibitor is selected from boric acid compounds.

[0025] In one embodiment of the present invention, the boric acid compound is selected from one or more of boric acid, sodium borate, potassium borate, aluminum borate and zinc borate.

[0026] In one embodiment of the present invention, the inorganic acid is selected from one or more of hydrochloric acid, phosphoric acid, hydrofluoric acid and hydroiodic acid.

[0027] In one embodiment of the present invention, the organic acid is selected from one or more of formic acid, acetic acid, propionic acid, oxalic acid, malonic acid, butyric acid, succinic acid, valeric acid and glutaric acid, and the organic acid has wettability and can achieve a leveling effect.

[0028] In one embodiment of the present invention, the leveling agent is selected from one or more of benzenesulfonic acid, fluorobenzenesulfonic acid, halogenated benzenesulfonic acid, trifluoromethylbenzenesulfonic acid and nitrobenzenesulfonic acid; further, the trifluoromethylbenzenesulfonic acid is selected from 2-(trifluoromethyl)benzenesulfonic acid (CAS No.: 229326-04-9) and / or 4-(trifluoromethyl)benzenesulfonic acid (CAS No.: 109787-11-3); the leveling agent is a compound containing a strong electron-withdrawing group and a sulfonic acid group on the benzene ring, and has a certain leveling effect. A stronger synergistic leveling effect can be achieved by compounding the leveling agent and an organic acid.

[0029] In one embodiment of the present invention, the surfactant is selected from one or more of bisphenol A polyoxyethylene ether, lauryl alcohol polyoxyethylene ether, secondary alcohol polyoxyethylene ether and nonylphenol polyoxyethylene ether; the surfactant is a non-ionic surfactant with a benzene ring and a fatty chain, and the HLB value is relatively small. Because the benzene ring and the fatty chain are both hydrophobic groups, the surfactant has better lipophilicity. In this case, it can play a solubilizing role in the dissolution of organic components.

[0030] In one embodiment of the present invention, the wetting agent is a fatty alcohol compound.

[0031] In one embodiment of the present invention, the fatty alcohol compound is selected from one or more of 1-propanol, 2-propanol, butanol, 1,2-propylene glycol, 1,3-propylene glycol, glycerol, butanediol and pentanediol.

[0032] The second object of the present invention is to provide a method for preparing the aluminum etching solution, comprising the following steps: stirring an inorganic acid, an organic acid, a corrosion inhibitor, a leveling agent, a surfactant, a wetting agent and water to obtain the aluminum etching solution.

[0033] The third object of the present invention is to provide an application of the aluminum etching solution in metal aluminum etching in electronic manufacturing process.

[0034] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. It should be understood that the specific embodiments are only used to explain the present invention, but the embodiments are not intended to limit the present invention.

[0035] In the present invention, unless otherwise explained, technical and scientific terms used in the present invention have the same meanings as commonly understood by those skilled in the art to which the present invention belongs.

[0036] In the present invention, unless otherwise stated, the term "and / or" used in the present invention includes any and all combinations of one or more of the associated listed items.

[0037] In the present invention, unless otherwise stated, the experimental methods used in the embodiments of the present invention are conventional methods unless otherwise stated, and the materials, reagents, etc. used are all commercially available unless otherwise stated.

[0038] In the present invention, unless otherwise stated, when the terms "comprise" and / or "include" are used in the specification of the present invention, it indicates the existence of the described features, integers, steps, operations, raw materials or components, but does not exclude the existence or addition of one or more other features, integers, steps, operations, raw materials, components or their combinations.

[0039] Example 1

[0040] The aluminum etching solution raw material components and mass fractions of the present embodiment are as follows:

[0041] Inorganic hydrochloric acid 10%, organic acid acetic acid 0.5%, corrosion inhibitor sodium borate 2%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 1.5%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 5%, and the balance is water.

[0042] The specific steps include:

[0043] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0044] Example 2

[0045] The aluminum etching solution raw material components and mass fractions of the present embodiment are as follows:

[0046] Inorganic hydrochloric acid 20%, organic acid acetic acid 0.5%, corrosion inhibitor sodium borate 2%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 1.5%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 5%, and the balance is water.

[0047] The specific steps include:

[0048] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0049] Example 3

[0050] The aluminum etching solution raw material components and mass fractions of the present embodiment are as follows:

[0051] Inorganic hydrochloric acid 20%, organic acid acetic acid 1%, corrosion inhibitor sodium borate 2%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 1.5%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 5%, and the balance is water.

[0052] The specific steps include:

[0053] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0054] Example 4

[0055] The aluminum etching solution raw material components and mass fractions of the present embodiment are as follows:

[0056] Inorganic hydrochloric acid 20%, organic acid acetic acid 1%, corrosion inhibitor sodium borate 2%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 1.5%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 10%, and the balance is water.

[0057] The specific steps include:

[0058] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0059] Example 5

[0060] The aluminum etching solution raw material components and mass fractions of the present embodiment are as follows:

[0061] Inorganic hydrochloric acid 20%, organic acid acetic acid 1%, corrosion inhibitor sodium borate 2%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 3%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 10%, and the balance is water.

[0062] The specific steps include:

[0063] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0064] Example 6

[0065] The aluminum etching solution raw material components and mass fractions of the present embodiment are as follows:

[0066] Inorganic hydrochloric acid 20%, organic acid acetic acid 1%, corrosion inhibitor sodium borate 1%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 3%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 10%, and the balance is water.

[0067] The specific steps include:

[0068] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0069] Example 7

[0070] The aluminum etching solution raw material components and mass fractions of the present embodiment are as follows:

[0071] Inorganic hydrochloric acid 20%, organic acid acetic acid 1%, corrosion inhibitor sodium borate 1%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 3%, surfactant nonylphenol polyoxyethylene ether-101.5%, wetting agent 1,2-propylene glycol 10%, and the balance is water.

[0072] The specific steps include:

[0073] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0074] Example 8

[0075] The aluminum etching solution raw material components and mass fractions of the present embodiment are as follows:

[0076] Inorganic acid phosphoric acid 20%, organic acid acetic acid 1%, corrosion inhibitor sodium borate 2%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 3%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 10%, and the balance is water.

[0077] The specific steps include:

[0078] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0079] Example 9

[0080] The aluminum etching solution raw material components and mass fractions of the present embodiment are as follows:

[0081] Inorganic hydrochloric acid 20%, organic acid propionic acid 1%, corrosion inhibitor sodium borate 2%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 3%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 10%, and the balance is water.

[0082] The specific steps include:

[0083] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0084] Example 10

[0085] The aluminum etching solution raw material components and mass fractions of the present embodiment are as follows:

[0086] Inorganic hydrochloric acid 20%, organic acid acetic acid 1%, corrosion inhibitor sodium borate 2%, leveling agent 2-fluorobenzenesulfonic acid 3%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 10%, and the balance is water.

[0087] The specific steps include:

[0088] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0089] Embodiment 11

[0090] The aluminum etching solution raw material components and mass fractions of the present embodiment are as follows:

[0091] Inorganic hydrochloric acid 20%, organic acid acetic acid 1%, corrosion inhibitor sodium borate 2%, leveling agent 4-(trifluoromethyl)benzenesulfonic acid 3%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 10%, and the balance is water.

[0092] The specific steps include:

[0093] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0094] Example 12

[0095] The aluminum etching solution raw material components and mass fractions of the present embodiment are as follows:

[0096] Inorganic hydrochloric acid 20%, organic acid acetic acid 1%, corrosion inhibitor potassium borate 2%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 3%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 10%, and the balance is water.

[0097] The specific steps include:

[0098] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0099] Example 13

[0100] The aluminum etching solution raw material components and mass fractions of the present embodiment are as follows:

[0101] Inorganic hydrochloric acid 20%, organic acid acetic acid 1%, corrosion inhibitor sodium borate 2%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 3%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent glycerol 10%, and the balance is water.

[0102] The specific steps include:

[0103] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0104] Embodiment 14

[0105] The aluminum etching solution raw material components and mass fractions of the present embodiment are as follows:

[0106] Inorganic hydrochloric acid 20%, organic acid acetic acid 1%, corrosion inhibitor sodium borate 2%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 3%, surfactant bisphenol A polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 10%, and the balance is water.

[0107] The specific steps include:

[0108] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0109] Comparative Example 1 is basically the same as Example 1 except that no inorganic hydrochloric acid is added.

[0110] The raw material components and mass fractions of the aluminum etching solution of this comparative example are as follows:

[0111] Organic acid acetic acid 0.5%, corrosion inhibitor sodium borate 2%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 1.5%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 5%, and the balance is water.

[0112] The specific steps include:

[0113] The organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0114] Comparative Example 2 is basically the same as Example 5 except that the inorganic hydrochloric acid is replaced with inorganic acid sulfuric acid. The raw material components and mass fractions of the aluminum etching solution in this comparative example are as follows:

[0115] Inorganic acid sulfuric acid 20%, organic acid acetic acid 1%, corrosion inhibitor sodium borate 2%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 3%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 10%, and the balance is water.

[0116] The specific steps include:

[0117] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0118] Comparative Example 3 is basically the same as Example 5 except that no corrosion inhibitor sodium borate is added.

[0119] The raw material components and mass fractions of the aluminum etching solution of this comparative example are as follows:

[0120] Inorganic hydrochloric acid 20%, organic acid acetic acid 1%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 3%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 10%, and the balance is water.

[0121] The specific steps include:

[0122] The inorganic acid, the organic acid, the leveling agent, the surfactant, the wetting agent and the water are stirred uniformly to obtain the aluminum etching solution.

[0123] Comparative Example 4 is basically the same as Example 5 except that the corrosion inhibitor sodium borate is replaced by the corrosion inhibitor sodium phosphate

[0124] The raw material components and mass fractions of the aluminum etching solution of this comparative example are as follows:

[0125] Inorganic hydrochloric acid 20%, organic acid acetic acid 1%, corrosion inhibitor sodium phosphate 2%, leveling agent 2-(trifluoromethyl)benzenesulfonic acid 3%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 10%, and the balance is water.

[0126] The specific steps include:

[0127] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0128] Comparative Example 5 is basically the same as Example 5 except that the leveling agent 2-(trifluoromethyl)benzenesulfonic acid is not added.

[0129] The raw material components and mass fractions of the aluminum etching solution of this comparative example are as follows:

[0130] Inorganic hydrochloric acid 20%, organic acid acetic acid 1%, corrosion inhibitor sodium borate 2%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 10%, and the balance is water.

[0131] The specific steps include:

[0132] The inorganic acid, the organic acid, the corrosion inhibitor, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0133] Comparative Example 6 is basically the same as Example 5 except that the leveling agent 2-(trifluoromethyl)benzenesulfonic acid is replaced by the leveling agent 1,2,4-triazole

[0134] The raw material components and mass fractions of the aluminum etching solution of this comparative example are as follows:

[0135] Inorganic hydrochloric acid 20%, organic acid acetic acid 1%, corrosion inhibitor sodium borate 2%, leveling agent 1,2,4-triazole 3%, surfactant nonylphenol polyoxyethylene ether-101%, wetting agent 1,2-propylene glycol 10%, and the balance is water.

[0136] The specific steps include:

[0137] The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are uniformly stirred to obtain the aluminum etching solution.

[0138] Test Case

[0139] (1) The aluminum etching solutions of Examples 1-14 and Comparative Examples 1-6 were subjected to etching tests by a weighing method, specifically comprising the following steps: immersing 5*5 cm pure aluminum sheets for 5 min at a temperature of 25° C., weighing the weight of aluminum before and after and calculating the difference, and finally calculating the aluminum etching rate according to the aluminum etching rate calculation formula; aluminum etching rate formula: v=△m(g) / {S(cm 2 )*t(min)*ρ(g / cm 3 )}*10000;

[0140] Where, v: metal etching rate, unit: μm / min;

[0141] △m: The difference in weight before and after metal etching, in g;

[0142] S: metal immersion area, unit: cm 2 ;

[0143] t: soaking time, unit: min;

[0144] ρ: metal density, unit: g / cm 3 ;

[0145] (2) A 40 μm thick aluminum-containing circuit was immersed in the aluminum etching solution of Examples 1-14 and Comparative Examples 1-6, respectively, and the circuit was etched to observe the uniformity after etching. A metallographic microscope*100 times was used for observation. The uniformity of the circuit was scored on a scale of 1-10, with 1 being the worst and 10 being the best. Corrosiveness to metal equipment: triangle ▲ indicates severe corrosion, square ■ indicates general corrosion, and circle ● indicates no corrosion;

[0146] Figure 1-Figure 2 This is an etching effect diagram;

[0147] Table 1 shows the final measured results:

[0148] Table 1

[0149] Sample Aluminum etching rate (μm / min) Uniformity Equipment corrosion Example 1 3.0 8 ● Example 2 3.6 7 ● Example 3 3.8 8 ● Example 4 3.8 9 ● Example 5 4 10 ● Example 6 3.9 10 ● Example 7 4 10 ● Example 8 3 10 ● Example 9 3.9 10 ● Example 10 4 10 ● Embodiment 11 4 9 ● Example 12 4 10 ● Example 13 4 10 ● Embodiment 14 4 10 ● Comparative Example 1 0.1 10 ● Comparative Example 2 0.5 10 ● Comparative Example 3 3.9 10 ▲ Comparative Example 4 3.8 10 ■ Comparative Example 5 3.6 1 ● Comparative Example 6 3.2 3 ●

[0150] from Figure 1-Figure 2 It can be seen from Table 1 that the aluminum etching solution of the embodiment has a high etching rate, which can reach up to about 4 μm / min; the etching is uniform, and the circuit after etching is relatively flat; during use, it will not cause serious corrosion problems on the surface of the equipment.

[0151] By comparing Examples 1-2 with Comparative Example 1, it can be seen that the content of inorganic hydrochloric acid affects the aluminum etching rate; by comparing Examples 5 and 8 with Comparative Example 2, it can be seen that the type of inorganic acid also has a relatively large effect on the aluminum etching rate. Compared with phosphoric acid and sulfuric acid, the atomic radius of the ligand chloride ion in hydrochloric acid is relatively small, and its penetration into aluminum metal is relatively strong, so the etching rate is slightly faster, and aluminum metal is easily passivated in high concentration sulfuric acid, which prevents further reaction.

[0152] Comparing Examples 2-4, it can be seen that both the organic acid and the wetting agent can increase the flatness by wetting the sample circuit, and the higher the organic acid content, the higher the aluminum etching rate.

[0153] Comparison of Examples 4-5, 10-11 and Comparative Examples 5-6 shows that the leveling agent has a very obvious effect on the aluminum circuit. At the same time, the higher its content, the aluminum etching rate will also increase slightly. However, its electron-withdrawing group is in the para position, and its flatness will be slightly worse. This is because its electron-withdrawing effect in the para position is relatively weak, and the electron cloud density of the sulfonic acid group is relatively large, so the proton ionization degree is low, resulting in a weak leveling effect. And if the traditional leveling agent uses triazole to level the corrosion inhibition performance of aluminum, the effect in this system is far less than adding compounds containing strong electron-withdrawing groups and sulfonic acid groups on the benzene ring.

[0154] By comparing Examples 5-6, 12 and Comparative Examples 3-4, it can be seen that the content and type of boric acid compounds have little effect on the corrosion inhibition performance of the equipment; phosphates, which are also used as pH adjusters, are obviously not as effective as borates in protecting equipment.

[0155] Comparing Examples 7-9 and 13-14, it can be seen that the type of organic acid, the type of wetting agent, the type of non-ionic surfactant and its content have no effect on the aluminum etching rate, flatness and equipment corrosion.

[0156] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. An aluminum etching solution, characterized in that: Calculated by weight, it includes 5%-20% of inorganic acid, 0.1%-1% of organic acid, 0.1%-2% of corrosion inhibitor, 0.5%-3% of leveler, 0.1%-1.5% of surfactant, 1%-10% of wetting agent, and the balance is water; the corrosion inhibitor is selected from boric acid compounds.

2. The aluminum etching solution according to claim 1, characterized in that The boric acid compound is selected from one or more of boric acid, sodium borate, potassium borate, aluminum borate and zinc borate.

3. The aluminum etching solution according to claim 1, characterized in that The inorganic acid is selected from one or more of hydrochloric acid, phosphoric acid, hydrofluoric acid and hydroiodic acid.

4. The aluminum etching solution according to claim 1, characterized in that The organic acid is selected from one or more of formic acid, acetic acid, propionic acid, oxalic acid, malonic acid, butyric acid, succinic acid, valeric acid and glutaric acid.

5. The aluminum etching solution according to claim 1, characterized in that: The leveler is selected from one or more of benzenesulfonic acid, fluorobenzenesulfonic acid, halogenated benzenesulfonic acid, trifluoromethylbenzenesulfonic acid and nitrobenzenesulfonic acid.

6. The aluminum etching solution according to claim 1, characterized in that: The surfactant is selected from one or more of bisphenol A polyoxyethylene ether, lauryl alcohol polyoxyethylene ether, secondary alcohol polyoxyethylene ether and nonylphenol polyoxyethylene ether.

7. The aluminum etching solution according to claim 1, characterized in that: The wetting agent is a fatty alcohol compound.

8. The aluminum etching solution according to claim 7, characterized in that: The fatty alcohol compound is selected from one or more of 1-propanol, 2-propanol, butanol, 1,2-propylene glycol, 1,3-propylene glycol, glycerol, butanediol and pentanediol.

9. A method for preparing an aluminum etching solution as claimed in any one of claims 1 to 8, characterized in that: The following steps are involved: The inorganic acid, the organic acid, the corrosion inhibitor, the leveler, the surfactant, the wetting agent and the water are stirred evenly to obtain the aluminum etching solution.

10. Use of the aluminum etching solution as claimed in any one of claims 1 to 8 in an electronic manufacturing process.

Citation Information

Cited By

  • Method for preparing nano silicon by etching silicon-aluminum alloy and nano silicon material thereof

    CN121651369A