CoFe-LDHs electrode material based on mechanochemical method as well as preparation method and application of CoFe-LDHs electrode material
The preparation of CoFe-LDHs electrode materials through mechanochemical method solved the problems of product agglomeration and low electrocatalytic activity, achieved electrode materials with good nano-size and dispersibility, significantly improved the catalytic performance in electrolytic water, and had important application prospects.
Patent Information
- Application Number
- CN202411127220.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art has problems such as easy agglomeration of the products, large particle size, uneven morphology and low electrocatalytic activity when preparing CoFe-LDHs electrode materials, which limits its performance in electrolytic water catalysis.
Using mechanochemical method, the Co source, Fe source, surfactant and dispersant are mixed for mechanochemical reaction, and the conditions are optimized to prepare nanoCoFe-LDHs electrode materials, and the agglomeration of reaction raw materials is avoided through the action of surfactant and dispersant, so as to achieve High dispersion and uniformity of the product.
The prepared CoFe-LDHs electrode material has small particle size, good dispersion and uniform morphology, which significantly improves the electrocatalytic activity, and exhibits a low oxygen evolution reaction potential during the electrolysis process in alkaline environment, close to commercial Pt/C -The performance of RuO2 catalyst has the advantages of high efficiency, environmental protection and low cost.
Smart Images

Figure CN118996482A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of hydrogen production by water electrolysis, and in particular to a CoFe-LDHs electrode material based on a mechanochemical method, and a preparation method and application thereof. Background Art
[0002] As an efficient hydrogen production process, water electrolysis is of great significance for promoting energy transformation and achieving sustainable development. However, the anodic oxygen evolution reaction (OER) in the water electrolysis process has become a key factor restricting the energy efficiency of the entire water electrolysis process due to its slow kinetics and high overpotential. Therefore, the development of efficient and low-cost water electrolysis catalysts is crucial to promote the development of the water electrolysis industry.
[0003] Layered double hydroxides (LDHs) have shown potential as water electrolysis catalysts due to their unique layered structure and adjustable chemical composition. LDHs not only have good electrochemical stability and excellent catalytic activity, but also have lower cost and abundant resources compared to traditional precious metal catalysts such as Pt and Ru, so they are regarded as ideal alternative materials. Although LDHs have great potential in the field of water electrolysis catalysts, the problems existing in their synthesis process limit the full realization of their performance. Although traditional synthesis methods such as hydrothermal method and co-precipitation method can prepare LDHs, they are often accompanied by problems such as product agglomeration, large particle size, and difficult to control morphology. These problems seriously affect the electrocatalytic activity and practical application of LDHs. Summary of the invention
[0004] The purpose of the present invention is to provide a CoFe-LDHs electrode material based on a mechanochemical method, a preparation method and an application thereof, so as to solve the problems that the product is easy to agglomerate, the particle size is large, the morphology is uneven and the electrocatalytic activity is low when preparing CoFe-LDHs by the existing synthesis method.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a CoFe-LDHs electrode material based on a mechanochemical method, comprising the following steps:
[0007] The Co source, the Fe source, the surfactant, the dispersant and water are mixed to carry out a mechanochemical reaction to obtain the CoFe-LDHs electrode material;
[0008] Wherein, the Co source is Co(OH)2, CoCl2 or CoSO4, and the Fe source is C6Fe2O 12 or Fe4(OH)2(SO4)5;
[0009] The rotation speed of the mechanochemical reaction is 300-600 rpm, the time is 1-6 hours, and the ball-to-material ratio is 50-100:1.
[0010] Preferably, in the preparation method of CoFe-LDHs electrode material based on mechanochemical method, the surfactant is one or two of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and hexadecyltrimethylammonium bromide; the dispersant is one or two of stearic acid, sodium stearate, polyethylene glycol and polymethyl methacrylate.
[0011] Preferably, in the method for preparing the CoFe-LDHs electrode material based on the mechanochemical method, the molar ratio of Co in the Co source to Fe in the Fe source is 0.5 to 4:1.
[0012] Preferably, in the method for preparing the CoFe-LDHs electrode material based on the mechanochemical method, the mass ratio of the Co source to the surfactant is 10 to 100:1.
[0013] Preferably, in the method for preparing CoFe-LDHs electrode material based on mechanochemical method, the mass ratio of the Co source to the dispersant is 20 to 80:1.
[0014] Preferably, in the method for preparing CoFe-LDHs electrode material based on a mechanochemical method, the mass ratio of the Co source to the water is 1 to 5:1.
[0015] The present invention also provides a CoFe-LDHs electrode material prepared by the preparation method.
[0016] The present invention also provides an application of the CoFe-LDHs electrode material in electrolyzing water.
[0017] Preferably, in the application of the CoFe-LDHs electrode material in water electrolysis, the electrode used for water electrolysis is coated with CoFe-LDHs slurry; the CoFe-LDHs slurry includes CoFe-LDHs electrode material, a conductive agent and a binder.
[0018] Preferably, in the application of the CoFe-LDHs electrode material in water electrolysis, the loading amount of the CoFe-LDHs electrode material on the electrode is 2 to 10 mg / cm 2 .
[0019] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) The present invention adopts a mechanochemical synthesis method, and on the basis of adding a Co source, an Fe source, a surfactant and a dispersant, optimizes the mechanochemical synthesis conditions, and finally prepares a highly dispersed nano CoFe-LDHs electrode material in one step. During the mechanochemical reaction, the surfactant and the dispersant work together to avoid the agglomeration of the reaction raw materials, promote more uniform mixing, contact and reaction of the solid raw materials, and make the product CoFe-LDHs have a small particle size, good dispersion and uniform morphology. Since the prepared CoFe-LDHs reach a nanometer size (5 to 50 nm) and are well dispersed, the catalytic area of the electrode material is large, and the exposed Co and Fe catalytic active sites are increased. Therefore, it exhibits good catalytic performance in the process of electrolysis of water in an alkaline environment, and at 10 mA / cm 2 When the current density is high, the potential of the oxygen evolution reaction (vs. RHE) is low, at 1.5-1.6 V, which is comparable to the catalytic performance of commercial Pt / C-RuO2 catalysts. This is of great strategic significance for promoting the development of the water electrolysis industry and realizing the green transformation of the energy structure.
[0021] (2) The main reagents used in the synthesis of CoFe-LDHs in the present invention are ferric oxalate, basic ferric sulfate, Co(OH)2, etc., and there is no need to add alkaline reagents such as NaOH and Na2CO3, which reduces the corrosion of equipment. 12 ) can decompose CO2 during the reaction, which is beneficial to the formation of LDHs layered structure; the water absorption of basic ferric sulfate (Fe4(OH)2(SO4)5) is beneficial to the formation of LDHs layered structure.
[0022] (3) The mechanochemical synthesis method of the present invention has the significant advantages of high efficiency, environmental protection and low cost, and has broad industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required to be used in the description of the embodiments or the prior art are briefly introduced below.
[0024] Figure 1 This is the XRD pattern of the CoFe-LDHs electrode material obtained in Example 1;
[0025] Figure 2 This is the SEM image of the CoFe-LDHs electrode material obtained in Example 1;
[0026] Figure 3 The oxygen evolution reaction test results of the CoFe-LDHs electrode material obtained in Example 1;
[0027] Figure 4 The XRD pattern of the CoFe-LDHs electrode material obtained in Comparative Example 1;
[0028] Figure 5 This is the SEM image of the CoFe-LDHs electrode material obtained in Comparative Example 1;
[0029] Figure 6 The XRD pattern of the CoFe-LDHs electrode material obtained in Comparative Example 2;
[0030] Figure 7 This is the SEM image of the CoFe-LDHs electrode material obtained in Comparative Example 2. DETAILED DESCRIPTION
[0031] The present invention provides a method for preparing a CoFe-LDHs electrode material based on a mechanochemical method, comprising the following steps:
[0032] The Co source, the Fe source, the surfactant, the dispersant and water are mixed to carry out a mechanochemical reaction to obtain the CoFe-LDHs electrode material;
[0033] Wherein, the Co source is Co(OH)2, CoCl2 or CoSO4, and the Fe source is C6Fe2O 12 or Fe4(OH)2(SO4)5;
[0034] The rotation speed of the mechanochemical reaction is 300-600 rpm, the time is 1-6 hours, and the ball-to-material ratio is 50-100:1.
[0035] In the present invention, the Co source is Co(OH)2, CoCl2 or CoSO4, preferably Co(OH)2 or CoCl2, and more preferably Co(OH)2.
[0036] In the present invention, the Fe source is C6Fe2O 12 or Fe4(OH)2(SO4)5, preferably C6Fe2O 12 .
[0037] In the present invention, the surfactant is preferably one or two of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and cetyltrimethylammonium bromide, more preferably sodium dodecyl sulfate, sodium dodecylbenzene sulfonate or cetyltrimethylammonium bromide, and more preferably sodium dodecyl sulfate.
[0038] In the present invention, the dispersant is preferably one or two of stearic acid, sodium stearate, polyethylene glycol and polymethyl methacrylate, more preferably one or two of stearic acid and sodium stearate, and more preferably stearic acid.
[0039] In the present invention, when the surfactant or the dispersant is preferably two kinds, the present invention does not limit the ratio between the two surfactants or the two dispersants, which can be adjusted according to needs.
[0040] In the present invention, the molecular weight of the polyethylene glycol is preferably 1,000 to 7,000,000, more preferably 1,000 to 200,000, and even more preferably 1,000.
[0041] In the present invention, the molecular weight of the polymethyl methacrylate is preferably 4,000 to 1,000,000, more preferably 20,000 to 250,000, and even more preferably 35,000.
[0042] In the present invention, the molar ratio of Co in the Co source to Fe in the Fe source is preferably 0.5 to 4:1, more preferably 0.5 to 2:1, and more preferably 0.5:1.
[0043] In the present invention, the mass ratio of the Co source to the surfactant is preferably 10 to 100:1, more preferably 10 to 40:1, and even more preferably 10:1.
[0044] In the present invention, the mass ratio of the Co source to the dispersant is preferably 20 to 80:1, more preferably 20 to 40:1, and more preferably 20:1.
[0045] In the present invention, the mass ratio of the Co source to the water is preferably 1 to 5:1, more preferably 1 to 2:1, and even more preferably 1:1.
[0046] In the present invention, the mechanochemical reaction method is preferably ball milling.
[0047] In the present invention, the equipment for the mechanochemical reaction is preferably a planetary ball mill.
[0048] In the present invention, the rotation speed of the mechanochemical reaction is 300-600rpm, preferably 300-450rpm, and more preferably 300rpm; the time is 1-6h, preferably 1-3h, and more preferably 1h; the ball-to-material ratio is 50-100:1, preferably 50-70:1, and more preferably 50:1.
[0049] The present invention also provides a CoFe-LDHs electrode material prepared by the preparation method.
[0050] The present invention also provides an application of the CoFe-LDHs electrode material in electrolyzing water.
[0051] In the present invention, the environment for electrolyzing water is preferably an alkaline environment.
[0052] In the present invention, the application method is not limited, and any method known to those skilled in the art may be used.
[0053] In the present invention, the electrode used for electrolysis of water is coated with CoFe-LDHs slurry.
[0054] In the present invention, the electrode used for electrolyzing water is preferably a graphite electrode.
[0055] In the present invention, the CoFe-LDHs slurry includes CoFe-LDHs electrode material, a conductive agent and a binder.
[0056] In the present invention, the conductive agent is preferably carbon black, conductive graphite, carbon nanotube or graphene, more preferably carbon black, conductive graphite or graphene, and more preferably carbon black.
[0057] In the present invention, the binder is preferably polyvinylidene fluoride, polyacrylate, polyvinyl alcohol, sodium carboxymethyl cellulose or polyimide, more preferably polyvinylidene fluoride, sodium carboxymethyl cellulose or polyimide, and more preferably polyvinylidene fluoride.
[0058] In the present invention, the molecular weight of the binder is not limited, and raw materials well known to those skilled in the art can be used.
[0059] In the present invention, the mass ratio of the CoFe-LDHs electrode material, the conductive agent and the binder is not limited and can be adjusted according to needs.
[0060] In the present invention, the loading amount of the CoFe-LDHs electrode material on the electrode is preferably 2 to 10 mg / cm 2 , more preferably 2 to 5 mg / cm 2 , more preferably 2 mg / cm 2 .
[0061] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0062] Example 1
[0063] This embodiment provides a method for preparing a CoFe-LDHs electrode material based on a mechanochemical method, comprising the following steps:
[0064] Co(OH)2、C6Fe2O 12, sodium dodecyl sulfate, stearic acid, and deionized water were added into a planetary ball mill and ball-milled for 1 hour at a rotation speed of 300 rpm and a ball-to-material ratio of 50:1 to carry out a mechanochemical reaction, wherein the molar ratio of Co to Fe is 0.5:1, the mass ratio of Co(OH)2 to sodium dodecyl sulfate is 10:1, the mass ratio of Co(OH)2 to stearic acid is 20:1, and the mass ratio of Co(OH)2 to deionized water is 1:1; after the reaction, the ball and material are separated to obtain CoFe-LDHs electrode material.
[0065] The CoFe-LDHs electrode material prepared in Example 1 was subjected to XRD detection, and the results were as follows: Figure 1 As shown. Figure 1 It can be seen that the diffraction peak of the CoFe-LDHs electrode material prepared in Example 1 corresponds to the PDF card number 40-0215, indicating that the layered double hydroxide was successfully synthesized based on the mechanochemical method.
[0066] The microscopic morphology of the CoFe-LDHs electrode material prepared in Example 1 is observed, and its SEM image is as follows: Figure 2 As shown. Figure 2 It can be seen that the CoFe-LDHs prepared in Example 1 mainly exist in the form of nanoparticles in a microscopic state, and the particle size is between 5 and 50 nm.
[0067] Application Example 1
[0068] The CoFe-LDHs electrode material prepared in Example 1, carbon black (Crode, ECP-600JD) and polyvinylidene fluoride (Crode, molecular weight 900) were prepared into an electrode slurry in a mass ratio of 8:1:1, and the slurry was coated on a graphite foil to obtain an electrode loaded with CoFe-LDHs. The loading amount of the CoFe-LDHs electrode material on the electrode was 2 mg / cm 2 In 3 mol / L KOH alkaline solution, the electrode loaded with CoFe-LDHs was used as the working electrode, graphite as the counter electrode, and Hg / HgO as the reference electrode. The results are as follows: Figure 3 As shown. Figure 3 It can be seen that at 10mA / cm 2At the current density, the potential of the oxygen evolution reaction (vs. RHE) is 1.55 V, which is close to the oxygen evolution voltage of Pt / C-RuO2 of 1.57 V disclosed in "Zn(II)-MOFs nanosheets interaction with P-doped graphitic carbon nitride nanosheets for effective overall water splitting in alkaline medium" (Krishnendu M. Nair et al., Journal of Electroanalytical Chemistry, DOI: 10.1016 / j.jelechem.2023.117968).
[0069] Example 2
[0070] This embodiment provides a method for preparing a CoFe-LDHs electrode material based on a mechanochemical method, comprising the following steps:
[0071] CoCl2、C6Fe2O 12 , sodium dodecylbenzene sulfonate, sodium stearate, and deionized water were added into a planetary ball mill and ball-milled for 2 hours at a rotation speed of 370 rpm and a ball-to-material ratio of 60:1 to carry out a mechanochemical reaction, wherein the molar ratio of Co to Fe is 1:1, the mass ratio of CoCl2 to sodium dodecylbenzene sulfonate is 30:1, the mass ratio of CoCl2 to sodium stearate is 35:1, and the mass ratio of CoCl2 to deionized water is 2:1; after the reaction, the ball and material are separated to obtain CoFe-LDHs electrode material.
[0072] Application Example 2
[0073] The CoFe-LDHs electrode material prepared in Example 2, conductive graphite (KS-6) and polyacrylate (Norton Laboratory Supplies Mall, molecular weight 676.84) were used to prepare an electrode slurry in a mass ratio of 8:1:1, and the slurry was coated on a graphite foil to obtain an electrode loaded with CoFe-LDHs. The loading amount of the CoFe-LDHs electrode material on the electrode was 4 mg / cm 2 In 3 mol / L KOH alkaline solution, the electrode loaded with CoFe-LDHs was used as the working electrode, graphite as the counter electrode, and Hg / HgO as the reference electrode. The test results were as follows: 2 At the current density, the potential of the oxygen evolution reaction (vs. RHE) is 1.55V.
[0074] Example 3
[0075] This embodiment provides a method for preparing a CoFe-LDHs electrode material based on a mechanochemical method, comprising the following steps:
[0076] Co(OH)2, Fe4(OH)2(SO4)5, hexadecyltrimethylammonium bromide, polyethylene glycol (molecular weight 1000), and deionized water were added together into a planetary ball mill and milled for 3 hours at a rotation speed of 440 rpm and a ball-to-material ratio of 70:1 to carry out a mechanochemical reaction, wherein the molar ratio of Co to Fe is 2:1, the mass ratio of Co(OH)2 to hexadecyltrimethylammonium bromide is 50:1, the mass ratio of Co(OH)2 to polyethylene glycol is 50:1, and the mass ratio of Co(OH)2 to deionized water is 3:1; after the reaction, the ball and material are separated to obtain CoFe-LDHs electrode material.
[0077] Application Example 3
[0078] The CoFe-LDHs electrode material prepared in Example 3, carbon nanotubes (McLean, G991390) and polyvinyl alcohol (McLean, molecular weight 9000) were mixed in a mass ratio of 8:1:1 to prepare an electrode slurry, which was coated on a graphite foil to obtain an electrode loaded with CoFe-LDHs. The loading amount of the CoFe-LDHs electrode material on the electrode was 6 mg / cm 2 In 3 mol / L KOH alkaline solution, the electrode loaded with CoFe-LDHs was used as the working electrode, graphite as the counter electrode, and Hg / HgO as the reference electrode. The test results were as follows: 2 At the current density, the potential of the oxygen evolution reaction (vs. RHE) is 1.54V.
[0079] Example 4
[0080] This embodiment provides a method for preparing a CoFe-LDHs electrode material based on a mechanochemical method, comprising the following steps:
[0081] CoSO4、C6Fe2O 12 , sodium dodecylbenzenesulfonate, polymethyl methacrylate (molecular weight 35000), and deionized water were added into a planetary ball mill and ball-milled for 4 hours at a rotation speed of 510 rpm and a ball-to-material ratio of 80:1 to carry out a mechanochemical reaction, wherein the molar ratio of Co to Fe is 3:1, the mass ratio of CoSO4 to sodium dodecylbenzenesulfonate is 70:1, the mass ratio of CoSO4 to polymethyl methacrylate is 65:1, and the mass ratio of CoSO4 to deionized water is 4:1; after the reaction, the ball and material are separated to obtain CoFe-LDHs electrode material.
[0082] Application Example 4
[0083] The CoFe-LDHs electrode material prepared in Example 4, graphene (McLean, G835835) and sodium carboxymethyl cellulose were prepared in a mass ratio of 8:1:1 to prepare an electrode slurry, which was coated on a graphite foil to obtain an electrode loaded with CoFe-LDHs. The loading amount of the CoFe-LDHs electrode material on the electrode was 8 mg / cm 2 In 3 mol / L KOH alkaline solution, the electrode loaded with CoFe-LDHs was used as the working electrode, graphite as the counter electrode, and Hg / HgO as the reference electrode. The test results were as follows: 2 At the current density, the potential of the oxygen evolution reaction (vs. RHE) is 1.58V.
[0084] Example 5
[0085] This embodiment provides a method for preparing a CoFe-LDHs electrode material based on a mechanochemical method, comprising the following steps:
[0086] CoCl2, Fe4(OH)2(SO4)5, cetyltrimethylammonium bromide, sodium dodecylbenzenesulfonate, polyethylene glycol (molecular weight 1000), polymethyl methacrylate (molecular weight 35000), and deionized water were added into a planetary ball mill and milled for 6 hours at a rotation speed of 600 rpm and a ball-to-material ratio of 100:1 for a mechanochemical reaction, wherein the molar ratio of Co to Fe was 4:1, the mass ratio of CoCl2 to the sum of the masses of cetyltrimethylammonium bromide + sodium dodecylbenzenesulfonate was 100:1 (the mass ratio of cetyltrimethylammonium bromide to sodium dodecylbenzenesulfonate was 1:1), the mass ratio of CoCl2 to the sum of the masses of polyethylene glycol + polymethyl methacrylate was 80:1 (the mass ratio of polyethylene glycol to polymethyl methacrylate was 1:2), and the mass ratio of CoCl2 to deionized water was 5:1; after the reaction, the balls and materials were separated to obtain CoFe-LDHs electrode material.
[0087] Application Example 5
[0088] The CoFe-LDHs electrode material prepared in Example 5, graphene (McLean, G835835) and polyimide (McLean, molecular weight 50000) were mixed in a mass ratio of 8:1:1 to prepare an electrode slurry, which was coated on a graphite foil to obtain an electrode loaded with CoFe-LDHs. The loading amount of the CoFe-LDHs electrode material on the electrode was 10 mg / cm 2 In 3 mol / L KOH alkaline solution, the electrode loaded with CoFe-LDHs was used as the working electrode, graphite as the counter electrode, and Hg / HgO as the reference electrode. The test results were as follows: 2 At the current density, the potential of the oxygen evolution reaction (vs. RHE) is 1.60V.
[0089] Comparative Example 1
[0090] This comparative example provides a method for preparing CoFe-LDHs electrode material by a hydrothermal method, comprising the following steps:
[0091] Weigh 1.5g CoCl2·6H2O, 0.50g FeCl3·6H2O, 0.05g Na3C6H5O7·2H2O and 1.5g H2NCONH2, dissolve in 90mL water, put into a 150mL reactor, react at 150℃ for 12h, wash three times after cooling, dry in a 70℃ forced air drying oven for 10h, and grind to obtain CoFe-LDHs electrode material.
[0092] The CoFe-LDHs electrode material prepared in Comparative Example 1 was subjected to XRD detection, and the results were as follows: Figure 4 As shown. Figure 4 It can be seen that the diffraction peak of the CoFe-LDHs electrode material prepared in Comparative Example 1 corresponds to the PDF card number 40-0215, indicating that the layered double hydroxide was successfully synthesized by the hydrothermal method.
[0093] The microscopic morphology of the CoFe-LDHs electrode material prepared in Comparative Example 1 is observed, and its SEM image is as follows: Figure 5 As shown. Figure 5 It can be seen that the CoFe-LDHs prepared in Comparative Example 1 also mainly exist in the form of nanoparticles in a microscopic state, with a particle size between 60 and 120 nm, but the particles have obvious agglomeration, adhesion, and merging.
[0094] Comparative application example 1
[0095] The CoFe-LDHs electrode material prepared in Comparative Example 1, carbon black (Crode, ECP-600JD) and polyvinylidene fluoride (Crode, molecular weight 900) were mixed in a mass ratio of 8:1:1 to prepare an electrode slurry, which was coated on a graphite foil to obtain an electrode loaded with CoFe-LDHs. The loading amount of the CoFe-LDHs electrode material on the electrode was 2 mg / cm 2 The test was carried out in 3 mol / L KOH alkaline solution with the electrode loaded with CoFe-LDHs as the working electrode, graphite as the counter electrode, and Hg / HgO as the reference electrode. 2 At the current density, the potential of the oxygen evolution reaction (vs. RHE) is 1.65V, which is higher than 1.55V in Example 1.
[0096] Comparative Example 2
[0097] This comparative example provides a method for preparing CoFe-LDHs electrode material by coprecipitation method, comprising the following steps:
[0098] Use an analytical balance to weigh 9.0g CoCl2·6H2O and 3.5g FeCl3·6H2O respectively and add them to a beaker, then add 50mL distilled water to dissolve them. Prepare 50mL of 2mol / LNaOH solution. Transfer the two solutions to the separatory funnels respectively and fix them with an iron stand. Place a beaker under the separatory funnel to collect the mixed solution produced during the titration process to ensure that the titration rate of the two separatory funnels is the same. After the titration is completed, take out the beaker below and seal it with a plastic film to prevent the solution from being disturbed by the outside. Then, let the beaker stand for 21h to allow the chemical reaction in the solution to proceed fully. The obtained product is first washed with deionized water and anhydrous ethanol by a centrifuge, and the centrifuge speed is set to 9000r / min. This washing process is repeated 3 times. The product needs to be resuspended after each washing to completely remove impurities. Subsequently, the washed product is transferred to a suction filter for suction filtration to further separate the solid product from the liquid. During the suction filtration process, the product is rinsed alternately with alcohol and water. After the filtration was completed, the product was transferred to a clean beaker and placed in a blast drying oven as a whole, and dried at a constant temperature of 70° C. for 10 h to obtain a CoFe-LDHs electrode material.
[0099] The CoFe-LDHs electrode material prepared in Comparative Example 2 was subjected to XRD detection, and the results were as follows: Figure 6 As shown. Figure 6 It can be seen that the diffraction peak of the CoFe-LDHs electrode material prepared in Comparative Example 2 corresponds to the PDF card number 40-0215, indicating that the layered double hydroxide was successfully synthesized by the co-precipitation method.
[0100] The microscopic morphology of the CoFe-LDHs electrode material prepared in Comparative Example 2 is observed, and its SEM image is as follows: Figure 7 As shown. Figure 7 It can be seen that the CoFe-LDHs prepared in Comparative Example 2 exist in the form of particles and rod-like structures in a microscopic state, and the morphology is not uniform.
[0101] Comparative Application Example 2
[0102] The CoFe-LDHs electrode material prepared in Comparative Example 2, carbon black (Crode, ECP-600JD) and polyvinylidene fluoride (Crode, molecular weight 900) were mixed in a mass ratio of 8:1:1 to prepare an electrode slurry, which was coated on a graphite foil to obtain an electrode loaded with CoFe-LDHs. The loading amount of the CoFe-LDHs electrode material on the electrode was 2 mg / cm 2 The test was carried out in 3 mol / L KOH alkaline solution with the electrode loaded with CoFe-LDHs as the working electrode, graphite as the counter electrode, and Hg / HgO as the reference electrode. 2At the current density, the potential of the oxygen evolution reaction (vs. RHE) is 1.69 V, which is higher than 1.55 V in Example 1.
[0103] Comparative Example 3
[0104] This comparative example provides a method for preparing a CoFe-LDHs electrode material based on a mechanochemical method, comprising the following steps:
[0105] Co(OH)2、C6Fe2O 12 , sodium dodecylbenzene sulfonate, sodium stearate and deionized water were added into a planetary ball mill and ball milled for 2 hours at a rotation speed of 370 rpm and a ball-to-material ratio of 60:1 to carry out a mechanochemical reaction, wherein the molar ratio of Co to Fe is 0.1:1, the mass ratio of Co(OH)2 to sodium dodecylbenzene sulfonate is 30:1, the mass ratio of Co(OH)2 to sodium stearate is 35:1, and the mass ratio of Co(OH)2 to deionized water is 2:1; after the reaction, the ball and material are separated to obtain CoFe-LDHs electrode material.
[0106] Comparative Application Example 3
[0107] The CoFe-LDHs electrode material prepared in Comparative Example 3, conductive graphite (KS-6) and polyacrylate (Norton Laboratory Supplies Mall, molecular weight 676.84) were used to prepare an electrode slurry in a mass ratio of 8:1:1, and the slurry was coated on a graphite foil to obtain an electrode loaded with CoFe-LDHs. The loading amount of the CoFe-LDHs electrode material on the electrode was 4 mg / cm 2 In 3 mol / L KOH alkaline solution, the electrode loaded with CoFe-LDHs was used as the working electrode, graphite as the counter electrode, and Hg / HgO as the reference electrode. The test results were as follows: 2 At the current density, the potential of the oxygen evolution reaction (vs. RHE) is 1.84V.
[0108] Comparative Example 4
[0109] This comparative example provides a method for preparing a CoFe-LDHs electrode material based on a mechanochemical method, comprising the following steps:
[0110] Co(OH)2、C6Fe2O 12, sodium dodecylbenzene sulfonate, sodium stearate and deionized water were added into a planetary ball mill and ball milled for 2 hours at a rotation speed of 370 rpm and a ball-to-material ratio of 60:1 to carry out a mechanochemical reaction, wherein the molar ratio of Co to Fe is 10:1, the mass ratio of Co(OH)2 to sodium dodecylbenzene sulfonate is 30:1, the mass ratio of Co(OH)2 to sodium stearate is 35:1, and the mass ratio of Co(OH)2 to deionized water is 2:1; after the reaction, the ball and material are separated to obtain CoFe-LDHs electrode material.
[0111] Comparative Application Example 4
[0112] The CoFe-LDHs electrode material prepared in Comparative Example 4, conductive graphite (KS-6) and polyacrylate (Norton Laboratory Supplies Mall, molecular weight 676.84) were used to prepare an electrode slurry in a mass ratio of 8:1:1, and the slurry was coated on a graphite foil to obtain an electrode loaded with CoFe-LDHs. The loading amount of the CoFe-LDHs electrode material on the electrode was 4 mg / cm 2 In 3 mol / L KOH alkaline solution, the electrode loaded with CoFe-LDHs was used as the working electrode, graphite as the counter electrode, and Hg / HgO as the reference electrode. The test results were as follows: 2 At the current density, the potential of the oxygen evolution reaction (vs. RHE) is 1.64V.
[0113] In summary, the present invention provides a mechanochemical method for preparing highly dispersed nano CoFe-LDHs electrode materials, and then the CoFe-LDHs electrode materials are uniformly coated on graphite foil to prepare electrodes that can be used for electrolysis of water and oxygen evolution reaction. Compared with the existing synthesis method of CoFe-LDHs electrode materials, the present invention adopts a mechanochemical method to prepare CoFe-LDHs electrode materials in one step, and the preparation method is simple and fast; at the same time, the product reaches nanometer size, good dispersibility, and good electrocatalytic performance, and has great application potential in the field of water electrolysis.
[0114] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing CoFe-LDHs electrode material based on mechanochemical method, characterized in that: The following steps are involved: The Co source, the Fe source, the surfactant, the dispersant and water are mixed to carry out a mechanochemical reaction to obtain the CoFe-LDHs electrode material; Wherein, the Co source is Co(OH)2, CoCl2 or CoSO4, and the Fe source is C6Fe2O 12 or Fe4(OH)2(SO4)5; The rotation speed of the mechanochemical reaction is 300-600 rpm, the time is 1-6 hours, and the ball-to-material ratio is 50-100:
1.
2. The method for preparing CoFe-LDHs electrode material based on mechanochemical method according to claim 1, characterized in that: The surfactant is one or two of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and cetyltrimethylammonium bromide; the dispersant is one or two of stearic acid, sodium stearate, polyethylene glycol and polymethyl methacrylate.
3. The method for preparing CoFe-LDHs electrode material based on mechanochemical method according to claim 1, characterized in that: The molar ratio of Co in the Co source to Fe in the Fe source is 0.5 to 4:
1.
4. A method for preparing a CoFe-LDHs electrode material based on a mechanochemical method as claimed in claim 1 or 2, characterized in that: The mass ratio of the Co source to the surfactant is 10 to 100:
1.
5. The method for preparing CoFe-LDHs electrode material based on mechanochemical method according to claim 4, characterized in that: The mass ratio of the Co source to the dispersant is 20 to 80:
1.
6. A method for preparing a CoFe-LDHs electrode material based on a mechanochemical method as claimed in claim 1 or 2, characterized in that: The mass ratio of the Co source to the water is 1 to 5:
1.
7. The CoFe-LDHs electrode material prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the CoFe-LDHs electrode material according to claim 7 in electrolysis of water.
9. Use of the CoFe-LDHs electrode material in electrolysis of water as claimed in claim 8, characterized in that: The electrode used for electrolyzing water is coated with CoFe-LDHs slurry; the CoFe-LDHs slurry comprises CoFe-LDHs electrode material, a conductive agent and a binder.
10. Use of the CoFe-LDHs electrode material in electrolysis of water according to claim 9, characterized in that: The loading amount of the CoFe-LDHs electrode material on the electrode is 2 to 10 mg / cm 2 .
Citation Information
Cited By
Preparation method of annealing-induced NO3-intercalated Ni-based LDH-coated FeOHSO4 oxygen evolution catalytic electrode