CoS-NiS / NCF catalyst and preparation method and application thereof

Through a brief one-step hydrothermal method, the CoS-NiS/NCF catalyst is synthesized, and the synergistic effect of Ni3S2 and Co9S8 is used to solve the problem of poor performance of non-precious metal dual-function electrocatalysts in the prior art, and efficient hydrogen and oxygen electrolysis is achieved reaction and surpass existing catalysts in stability and current density.

CN118996499APending Publication Date: 2024-11-22ZHEJIANG SCI-TECH UNIV

Patent Information

Application Number
CN202410978637.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing technology lacks efficient, economical and stable non-precious metal dual-function electrocatalysts, making it difficult to achieve efficient electrochemical water decomposition of hydrogen and oxygen in alkaline electrolytes at the same time, and transition metal chalcogenide compounds are compared with noble metal catalysts in terms of performance. There is a significant gap.

Method used

CoS-NiS/NCF catalyst was synthesized by a brief one-step hydrothermal method, using a needle-shaped leaf morphology structure, and using the synergistic action of Ni3S2 and Co9S8, the electrochemical surface area and active sites of the catalyst were improved, achieving efficient hydrogen gas and oxygen electrolysis.

Benefits of technology

The catalyst exhibits performance comparable to commercial Pt/C and RuO2 in both HER and OER, with higher stability and greater current density, and can be used as a replacement for precious metal electrolytic catalysts in the field of renewable energy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996499A_ABST
    Figure CN118996499A_ABST
Patent Text Reader

Abstract

The invention discloses a CoS-NiS / NCF catalyst and a preparation method and application thereof, and relates to the technical field of catalysts.The preparation method comprises the steps that S1, NiCo foam is cleaned up and aired for use; s2, ammonium fluoride, urea and S powder are mixed with deionized water, and then the mixed solution is stirred for a period of time and then subjected to ultrasonic treatment; s3, putting the NiCo foam in the step S1 and the mixed solution in the step S2 into a reaction kettle to react for a period of time; and S4, after the reaction is completed, taking out the NiCo foam, cleaning and drying to obtain the CoS-NiS / NCF catalyst. The bifunctional sulfide electrolyzed water catalyst has the beneficial effects that the bifunctional sulfide electrolyzed water catalyst is synthesized through a simple one-step hydrothermal method, the bifunctional sulfide electrolyzed water catalyst is of a needle-shaped nanostructure of pine tree leaves, and the bifunctional sulfide electrolyzed water catalyst has an efficient HER and OER bifunctional electrocatalytic material and has higher stability and higher current density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalysts, and in particular to a CoS-NiS / NCF catalyst and a preparation method and application thereof. Background Art

[0002] As hydrogen is regarded as an ideal clean fuel with excellent energy storage density, it is increasingly seen as a promising alternative to fossil fuels. Electrochemical water splitting has become a key method for large-scale hydrogen production, providing a way to solve energy shortages and environmental pollution. However, the efficiency of water splitting depends critically on minimizing the overpotentials of the cathode hydrogen evolution reaction (HER) and the anode oxygen evolution reaction (OER). Although the theoretical minimum voltage required for water splitting is 1.23V, commercial electrolyzers typically require higher voltages of about 1.8 to 2.0V due to the existence of overpotentials. To reduce these overpotentials, electrocatalysts are used, among which Pt-based metals are most active for HER, while IrO2 and RuO2 are used for OER. Although these catalysts are effective, they are limited by scarcity and high cost, so alternatives are needed to achieve widespread adoption. In addition, the reaction conditions, especially the acidity of the electrolyte, significantly affect the performance of the catalyst. Alkaline water splitting has become a strong candidate for commercial applications, emphasizing the need for catalysts compatible with such conditions. Furthermore, as the world shifts toward renewable energy sources such as wind, hydro, and solar, the need for efficient water electrolysis becomes more pressing, driving the need for non-precious metal electrocatalysts with high activity and durability to pave the way for sustainable hydrogen production.

[0003] Developing efficient and affordable catalysts for both hydrogen evolution reaction and oxygen evolution reaction in alkaline electrolytes is a key aspect in advancing electrochemical water splitting technology. Many non-noble metal-based catalysts, including cobalt- and nickel-based compounds such as CoOx@CN, PCPTF, and NiCo2S4 NA / CC, have been explored to realize their potential in water splitting. However, many challenges remain, such as the energy-intensive preparation process required for some catalysts. In addition, although transition metal chalcogenides (TMCs) have shown potential due to their excellent catalytic performance and low cost, there is still a significant performance gap compared with noble metal-based catalysts. Although efforts have been made to explore various TMCs such as sulfides, selenides, and phosphides, relatively little research attention has been paid to providing synergistic heterointerface engineering of two sulfides. Engineering bifunctional electrocatalysts for water splitting, especially in alkaline media, remains a great challenge, with few materials showing high activity and stability. In addition, the mismatch in reaction processes and coordinated reaction potentials makes it more complicated to integrate separate HER and OER catalysts into a single electrolyzer. Although some cobalt- or nickel-based catalysts have shown promise in catalyzing both reactions, they often exhibit lower activity and stability than their noble metal-based counterparts and require higher voltages for water splitting. Addressing these challenges and developing efficient bifunctional electrocatalysts could drive advances in energy systems and reduce production costs, ultimately facilitating the integration of water splitting technology into sustainable energy infrastructure.

[0004] At present, relevant studies have shown that Ni3S2 is a promising metal chalcogenide water electrolysis catalyst, which can be used for HER and OER, but there are few reports on water electrolysis catalyst materials with high efficiency of HER and OER. At the same time, there are some reports on Co9S8 for efficient OER catalysis, but there are few reports on its efficient HER. Summary of the invention

[0005] The purpose of the present invention is to solve at least one of the technical problems existing in the prior art and to provide a CoS-NiS / NCF catalyst and a preparation method and application thereof.

[0006] The present invention synthesizes a bifunctional sulfide electrolytic water catalyst through a short one-step method. Through morphological analysis, the present invention synthesizes a needle-like leaf morphology composed of small particles. This layered needle-like leaf can greatly increase the electrochemical surface area of ​​the catalyst, thereby increasing the current density of the catalyst. At the same time, through phase analysis, we cleverly synthesized two active substances, Ni3S2 and Co9S8, for HER activity and OER activity respectively, and their combined action can improve the corresponding HER and OER performance.

[0007] The technical solution of the present invention is as follows:

[0008] The first aspect of the present invention provides a method for preparing a CoS-NiS / NCF catalyst, comprising the following steps:

[0009] S1. Clean the NiCo foam and dry it for later use;

[0010] S2, mixing ammonium fluoride, urea and S powder with deionized water, and then stirring the mixed solution for a period of time, and then performing ultrasonic treatment;

[0011] S3, placing the NiCo foam in step S1 and the mixed solution in step S2 into a reactor to react for a period of time;

[0012] S4. After the reaction is completed, the NiCo foam is taken out, cleaned and dried to obtain a CoS-NiS / NCF catalyst.

[0013] Preferably, step S1 specifically includes:

[0014] The NiCo foam was placed in an acetone solution and subjected to ultrasonic treatment; after the ultrasonic treatment, the acetone on the surface of the NiCo foam was cleaned with ethanol and deionized water respectively; then the NiCo foam was placed in an HCl solution and subjected to ultrasonic treatment; after the ultrasonic treatment, the acetone on the surface of the NiCo foam was cleaned with ethanol and deionized water respectively, and the solution was dried for later use.

[0015] Preferably, in step S1, the power of the two ultrasonic treatments is 50-70 W, and the ultrasonic time is 8-12 min.

[0016] Preferably, in step S2, the mass ratio of ammonium fluoride, urea and S powder is 200-250:450-500:58-98.

[0017] Preferably, in step S2, the mixed solution is stirred at a rotation speed of 800 to 1200 rpm for 8 to 12 minutes.

[0018] Preferably, in step S2, ultrasound is performed at a power of 80 to 120 W for 8 to 12 minutes.

[0019] Preferably, in step S3, the reaction is carried out at a temperature of 140 to 170° C. for 4 to 9 hours.

[0020] Preferably, in step S4, the NiCo foam is dried at 40-60° C. for 1.5-2.5 h.

[0021] The second aspect of the present invention provides a CoS-NiS / NCF catalyst obtained by the above method.

[0022] A second aspect of the present invention provides use of the CoS-NiS / NCF catalyst in hydrogen production.

[0023] The present invention has at least one of the following beneficial effects:

[0024] The present invention synthesizes a bifunctional sulfide water electrolysis catalyst through a simple one-step hydrothermal method. The catalyst is a needle-shaped nanostructure of pine leaves. Through a series of characterizations, it is found that its main active sites come from Ni3S2 and Co9S8. Therefore, the material has both efficient HER and OER bifunctional electrocatalytic materials, which is comparable to the commercial HER catalyst Pt / C and the commercial OER catalyst RuO2. In addition, the material has higher stability and greater current density, and is expected to become one of the alternative precious metal water electrolysis catalytic materials in the field of hydrogen production in the field of renewable energy.

[0025] Compared with the nanostructure in the prior art, the needle-shaped leaf structure of the present invention can greatly increase the specific surface area of ​​the catalyst material and expose more active sites. At the same time, the synergy of the two active substances Ni3S2 and Co9S8 further improves their respective HER and OER performances.

[0026] The present invention adopts 10 and j 1000 The overpotential at 100 mA cm / s was used to characterize the HER and OER performances, where HER achieved excellent performances of 59 mV and 328 mV, and OER also achieved excellent performances of 98 mV and 423 mV. At the same time, the stability of the sulfide catalysts in the prior art is relatively poor. The catalyst synthesized by the present invention has good stability under the condition of 100 mA cm / s for 50 h. -2 HER stability test and 50h 200mA cm -2 After the stability test, the activity of Ni3S2 and Co9S8 did not decay.

[0027] In summary, the present invention provides a new scheme for synthesizing non-precious metal water electrolysis catalyst materials, which have efficient HER and OER bifunctional electrocatalytic materials with higher stability and greater current density. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a flow chart for preparing the CoS-NiS / NCF electrode material in Examples 1 to 3.

[0029] Figure 2 The figures are test diagrams of the effects of different foams on the performance of catalysts in Example 1 and Comparative Examples 1-2. Among them, (a) HER polarization curve, (b) HER Tafel diagram, (c) HER impedance diagram, (d) OER polarization curve, (e) OER Tafel diagram, (f) OER impedance diagram.

[0030] Figure 3 The figures are test diagrams of the effects of different sulfur powder masses on the performance of the catalysts in Examples 1 to 3. Among them, (a) HER polarization curve, (b) HER Tafel diagram, (c) HER impedance diagram, (d) OER polarization curve, (e) OER Tafel diagram, and (f) OER impedance diagram.

[0031] Figure 4 The effects of different reaction times on the performance of the catalysts in Examples 1 to 3 are shown in Figures 1 to 3. (a) HER polarization curve, (b) HER Tafel plot, (c) HER impedance plot, (d) OER polarization curve, (e) OER Tafel plot, and (f) OER impedance plot.

[0032] Figure 5 The effects of different reaction temperatures on the performance of the catalysts in Examples 1 to 2 are shown in Figures 1 and 2. (a) HER polarization curve, (b) HER Tafel plot, (c) HER impedance plot, (d) OER polarization curve, (e) OER Tafel plot, and (f) OER impedance plot.

[0033] Figure 6 This is a physical picture of the catalyst prepared in Comparative Example 3.

[0034] Figure 7 It is the XRD diagram of the catalysts prepared in Example 1 and Comparative Examples 1-2 after sulfurization.

[0035] Figure 8 The SEM morphology of the catalyst prepared in Example 1. (a) and (b) are SEM images at different magnifications, and (c) is SEM mapping.

[0036] Fig. 9 The TEM morphology of the catalyst prepared in Example 1 is shown in Figure 1. (a) and (b) are TEM high-resolution crystal plane images, and (c) is a TEM SAED image.

[0037] Fig.10 This is the XPS morphology of the catalyst prepared in Example 1. Among them, (a) Co 2p, (b) Ni 2p, (c) S2p, and (d) O 1s.

[0038] Fig.11 The HER electrochemical performance diagrams of the catalysts prepared in Example 1 and Comparative Examples 1 to 2 include (a) polarization curve, (b) Tafel slope, (c) impedance, (d) mass activity, (e) conversion frequency, and (f) Tafel-overpotential comparison.

[0039] Fig.12The OER electrochemical performance diagrams of the catalysts prepared in Example 1 and Comparative Examples 1 to 2 include (a) polarization curve, (b) Tafel slope, (c) impedance, (d) mass activity, (e) conversion frequency, and (f) Tafel-overpotential comparison.

[0040] Fig.13 The catalysts obtained in Example 1 and Comparative Examples 1 to 2 are C dl Among them, (a) CV graph of nickel-cobalt alloy foam, (b) C graph of nickel-cobalt alloy foam dl , (c) CV graph of nickel foam, (d) nickel foam C dl , (e) Cobalt foam CV graph, (f) Cobalt foam C dl .

[0041] Fig.14 The stability test graph of the catalyst prepared in Example 1. (a) The polarization curve of HER before and after 10,000 CV cycles, (b) The polarization curve of OER before and after 10,000 CV cycles, (c) HER 100 mA cm -2 50 h It stability test, (d) OER 200 mA cm -2 50h IT stability test. DETAILED DESCRIPTION

[0042] The present invention is further described in detail below with specific examples, but the present invention is not limited to the following specific examples.

[0043] The "NiCo foam" in the following examples is a nickel-cobalt alloy foam, in which the molar ratio of nickel to cobalt is 2:8, purchased from Suzhou Taili Foam Metal Factory, and has a thickness of 1 mm. The "Ni foam" in Comparative Example 1 and the "Co foam" in Comparative Example 2 were purchased from Suzhou Taili Foam Metal Factory, and have a thickness of 1 mm.

[0044] Example 1 Preparation of CoS-NiS / NCF

[0045] (1) Foam cleaning: Place 1×1cm 2 The NiCo foam was placed in a beaker containing 20mL of acetone solution, and then the beaker was placed in an ultrasonic machine and ultrasonicated at a power of 60W for 10min. After the ultrasonication, the acetone on the surface of the NiCo foam was cleaned with ethanol and deionized water respectively. The NiCo foam was then placed in a beaker containing 20mL of HCl solution (1M) and ultrasonicated at a power of 60W for 10min. After the ultrasonication, the acetone on the surface of the NiCo foam was cleaned with ethanol and deionized water respectively, and then naturally dried for use.

[0046] (2) Prepare the reaction solution: Weigh 225 mg of ammonium fluoride, 480 mg of urea and 78 mg of S powder respectively. Then mix the weighed drugs with 20 mL of deionized water. Then stir the mixed solution at 1000 rpm for 10 min, and then ultrasonicate at 100 W for 10 min.

[0047] (3) Reaction: The prepared mixed solution and NiCo foam were placed in a polytetrafluoroethylene reactor, and then the reactor was placed in an oven and reacted at 160° C. for 6 h.

[0048] (4) Drying: After the reaction is completed, the NiCo foam is taken out and rinsed with deionized water and ethanol three times. Then, the NiCo foam is placed in an oven and dried at 50°C for 2 h.

[0049] Example 2 Preparation of CoS-NiS / NCF

[0050] The difference from Example 1 is that the reaction temperature and time in step (3) are changed to "140°C for 9h".

[0051] Example 3 Preparation of CoS-NiS / NCF

[0052] The difference from Example 1 is that the reaction temperature and time in step (3) are changed to "170° C. for 4 hours".

[0053] Comparative Example 1 Preparation of NiS / NF

[0054] The difference from Example 1 is that the "NiCo foam" in step (1) is replaced by "Ni foam".

[0055] The rest is the same as Example 1.

[0056] Comparative Example 2 Preparation of CoS / CF

[0057] The difference from Example 1 is that the "NiCo foam" in step (1) is replaced by "Co foam".

[0058] The rest is the same as Example 1.

[0059] Comparative Example 3

[0060] The difference from Example 1 is that the "reaction temperature of 160° C." in step (3) is replaced by "reaction temperature of 180° C.", and the rest is the same as Example 1.

[0061] Testing and analysis

[0062] The catalysts prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were subjected to the following performance tests.

[0063] 1. CoS-NiS / NCF parameter exploration

[0064] (1) Foam Type

[0065] First, in order to select suitable foam as the substrate, we selected three foams for parameter exploration. The three foams are nickel foam (Comparative Example 1), cobalt foam (Comparative Example 2) and nickel-cobalt alloy foam (Example 1). The three different foams were vulcanized using the same experimental parameters. After the reaction, 0.5 cm x 0.5 cm samples were taken for electrochemical testing, and their performance was evaluated from three opposite sides: polarization curve, Tafel slope and impedance.

[0066] Figure 2 (a) is the HER polarization curve of the three foams. In the figure, we find that the performance of Co foam (Comparative Example 2) is the worst. At the same time, it has a huge reduction peak at low current, while nickel foam (Comparative Example 1) and nickel-cobalt alloy foam (Example 1) do not have this. Among them, the performance of nickel-cobalt alloy foam is the best.

[0067] Figure 2 (d) is the OER polarization curve of the three foams. In the figure, we find that the Ni foam has the worst performance and has an obvious oxidation peak. Although the Ni-Co alloy foam has a low current of 10 mA cm -2 The overpotential of the nickel-cobalt alloy foam is not as good as that of the cobalt foam, but the high current of 1000 mA cm -2 It is better than cobalt foam.

[0068] Figure 2 (b) and (e) are the Tafel slopes of HER and OER of the three foams. In contrast, the nickel-cobalt alloy foam has a lower Tafel slope, with a HER of 49.4 mVdec. -2 , OER is 65.4mVdec -2 .

[0069] Figure 2 (c) and (f) are the impedance diagrams of HER and OER of the three foams. Whether it is the impedance diagram of HER or OER, the nickel-cobalt alloy foam has smaller Rs and Rct.

[0070] Based on the above three aspects of performance evaluation, the present invention selects nickel-cobalt alloy foam as the most optimal reaction substrate.

[0071] (2) In order to further improve the catalytic performance, the present invention also studies the effect of different sulfur powder usage qualities on the catalyst performance.

[0072] Figure 3(a) and (d) are the corresponding HER and OER polarization curves, respectively. We found that no matter HER or OER, the use of 78 mg sulfur powder has lower small current overpotential and large current overpotential.

[0073] Figure 3 (b) and (e) are the Tafel slopes of HER and OER, respectively. By comparison, it is found that the sulfur powder with a mass of 78 mg has a lower Tafel slope, HER is 42.6 mV dec. -2 , OER is 65.4mV dec -2 .

[0074] exist Figure 3 In (c) and (f), the parameters of 78 mg sulfur powder in the impedance diagrams of HER and OER have lower Rs and Rct.

[0075] Therefore, through the above three performance evaluations, compared with Example 2 and Example 3, the 78 mg sulfur powder selected in Example 1 is the best reaction sulfur powder mass.

[0076] (3) After determining the mass of the sulfur powder, the present invention explores the reaction time.

[0077] exist Figure 4 In the polarization curves of HER and OER in (a) and (d), the reaction time of 6 h has the best performance.

[0078] Figure 4 (b) and (e) are the Tafel slopes of HER and OER. The 6 h reaction time has the lowest Tafel slope, with HER and OER being 49.2 mVdec, respectively. -2 and 79.6mVdec -2 .

[0079] In impedance comparison Figure 4 In (c) and (f), the reaction time of 6 h has the lowest Rs and Rct.

[0080] Therefore, according to the above results, compared with Example 2 and Example 3, the 6h reaction time selected in Example 1 is the best experimental parameter.

[0081] (4) The present invention also explores the effect of reaction temperature on catalyst performance.

[0082] Figure 6 This is a picture of the sample obtained by reaction at 180°C in Example 3. We found that the sample was very fragile and could not be used as a suitable electrode for performance testing, so there is no electrochemical data at 180°C.

[0083] exist Figure 5(a) and (d) are the polarization curves of OER and HER at different temperatures. We found that the performance deteriorated after lowering the temperature, while increasing the temperature could improve the performance. However, further increasing the temperature would cause the sample to break. Therefore, a reaction temperature of 160°C has the best performance.

[0084] Figure 5 (b) and (e) are the Tafel slopes of HER and OER. The reaction temperature of 160 °C has a lower Tafel slope, which is 49.7 mVdec for HER and OER, respectively. -2 and 77.9mVdec -2 .

[0085] In impedance comparison Figure 5 In (c) and (f), both HER and OER have lower Rs and Rct at a reaction temperature of 160 °C.

[0086] Therefore, since further increasing the temperature will cause the sample to break, compared with Example 2, Example 1 selects 160° C. as the most optimal reaction temperature.

[0087] 2. Phase analysis of CoS-NiS / NCF

[0088] In order to explore the main activity of the catalyst, the present invention performs XRD test on the samples prepared from the three foams of Example 1 and Comparative Examples 1-2.

[0089] Figure 7The following are the XRD results of three samples and the corresponding standard cards. The cyan line is the result of sulfurization of cobalt foam, where 29.82°, 31.18°, 47.55° and 52.06° correspond to the diffraction peaks of (311), (222), (511) and (440) crystal planes on the Co9S8 standard PFD card 73-1442, respectively. Therefore, it can be confirmed that the main active material on the cobalt foam is Co9S8. The red line is the result of sulfurization of nickel foam, where 31.27°, 31.98°, 35.446°, 40.231° and 55.3°4 correspond to the diffraction peaks of (311), (132), (312), (114) and (404) crystal planes on the Ni9S8 standard PFD card 78-1886. At the same time, 31.10°, 37.79°, 44.34°, 49.72°, 50.12°, 55.35° and 73.04° correspond to the diffraction peaks of (-110), (111), (020), (120), (-120), (-121) and (130) crystal planes on the Ni3S2 standard PFD card 71-1682. Therefore, it can be confirmed that the main active materials on the nickel foam are Ni9S8 and Ni3S2. The green line is the result of the vulcanization of the nickel-cobalt alloy foam, where 29.82°, 31.18°, 47.55° and 52.06° correspond to the diffraction peaks of (311), (222), (511) and (440) crystal planes on the Co9S8 standard PFD card 73-1442, respectively, while 31.10°, 44.34°, 49.72°, 50.112° and 73.04° correspond to the diffraction peaks of (-110), (020), (120), (-120) and (130) crystal planes on the Ni3S2 standard PFD card 71-1682. Therefore, it can be confirmed that the main active materials on the nickel-cobalt alloy foam are Co9S8 and Ni3S2.

[0090] Through the above results, it is found that the nickel-cobalt alloy foam retains the Co9S8 active material compared with the cobalt foam, and in recent literature reports, Co9S8 can be used as a highly active material for OER. Comparing the nickel-cobalt alloy foam with the nickel foam, we found that the nickel-cobalt alloy foam did not retain Ni9S8. The addition of the Co element may be the reason why Ni9S8 is generated on the nickel foam but not on the nickel-cobalt alloy foam. In recent literature reports, Ni3S2 is used as a highly active material for HER, but there are few literature reports related to Ni9S8. The introduction of the Co element inhibits the generation of Ni9S8 and improves the HER performance of the sample.

[0091] By comparison, we found that Figure 2In the nickel foam polarization curves in (a) and (d), the reduction peak of HER and the oxidation peak of OER may also be caused by the presence of Ni9S8. Therefore, through the above analysis, the main active materials in the CoS-NiS / NCF sample are Co9S8 and Ni3S2, among which Co9S8 is the main active material of OER and Ni3S2 is the main active material of HER.

[0092] 3. CoS-NiS / NCF morphology and structure analysis

[0093] (1) In order to explore the effect of the morphology and structure of the CoS-NiS / NCF catalyst on its performance, the present invention conducted SEM tests on the CoS-NiS / NCF samples.

[0094] Figure 8 (a) and (b) are SEM images of the samples at different magnifications. Figure 8 In (a), we can see many layers of pine needle-like leaves stacked together. Compared with the nanosheet morphology reported in many existing articles, it can increase its specific surface area. The leaf-like morphology is stacked layer by layer to fill the entire space. Figure 8 (b) is a morphology image with a larger magnification. We can clearly see that each leaf is grown from small particles one by one. These small particles are about a few hundred nanometers, and these tiny nanoparticles further increase the specific surface area of ​​the catalyst on the basis of the original layered leaves. The increase in specific surface area can increase the current density of the catalyst on the one hand, and expose more active sites on the other hand, thereby further improving the electrolytic water performance of CoS-NiS / NCF. Figure 8 (c) is the mapping test diagram. From the diagram, we can see that the distribution of elements in the whole leaf is very uniform. We can also find in Table 1 that the contents of sulfur, cobalt and nickel are basically close, and the content of oxygen is very small. This is consistent with our previous XRD results. The main active materials of the catalyst are Co9S8 and Ni3S2. At the same time, this shows that the catalyst we synthesized has good uniformity. Co9S8 and Ni3S2 are well combined. There may be a heterojunction to a certain extent, which enables them to cooperate with each other and thus improve the electrolytic water performance of the catalyst.

[0095] Table 1 shows the content of each element in the SEM mapping test

[0096]

[0097] (2) In order to explore the main catalytic crystal surface of the CoS-NiS / NCF catalyst, we performed TEM tests on the samples.

[0098] Fig. 9 (a) and (b) are high-resolution TEM images. In 9(a), we observed that the crystal plane with a crystal plane spacing of 0.238nm can be attributed to the (111) crystal plane of Ni3S2, and the crystal plane with a crystal plane spacing of 0.175nm can be attributed to the (440) crystal plane of Co9S8, and they form a heterogeneous interface. In 9(b), we observed that the crystal plane with a crystal plane spacing of 0.238nm can be attributed to the (111) crystal plane of Ni3S2 and the crystal plane with a crystal plane spacing of 0.286nm can be attributed to the (222) crystal plane of Co9S8, and they also form a heterogeneous interface. Fig. 9 (c) is the SAED test of TEM, and the obvious lattice diffraction found just corresponds to the previous crystal plane. The formation of heterogeneous interfaces can alleviate some stress in the crystal material to some extent, which plays an important role in regulating the catalytic active sites. In addition, we speculate that the reason why the performance of nickel-cobalt alloy foam is improved compared with that of single nickel foam and cobalt foam may be the synergistic effect brought about by these two sets of heterogeneous interfaces.

[0099] 4. Analysis of CoS-NiS / NCF valence state

[0100] In order to analyze the valence state of CoS-NiS / NCF, we performed XPS tests on the samples.

[0101] Fig.10 (a) is Co 2p High-resolution XPS graph of Co 2p Fitting into two different peaks and two weak satellite peaks, the two spin-orbit doublets at 780.8 eV and 795.9 eV can be attributed to Co 2p(3 / 2) and Co 2p(1 / 2) .Co 2p(3 / 2) It can be deconvoluted into two orbitals, 780.8eV and 782.3eV, which can be attributed to Co 3+ 2p(3 / 2) and Co 2+ 2p(3 / 2) . Also located in Co 2p(1 / 2) It can be deconvoluted into two orbitals, 795.8eV and 797.4eV, which can be attributed to Co 3+ 2p(1 / 2) and Co 2+ 2p(1 / 2) The two satellite peaks with binding energies of 788.2 eV and 804.8 eV can be attributed to surface oxidation.

[0102] Fig.10 (b) is Ni 2p The high-resolution XPS pattern of Ni2p(1 / 2) and Ni 2p(3 / 2) Two peaks and two oscillating satellite peaks, which can be deconvoluted into the 855.1 eV and 872.8 eV peaks of Ni 2+ and the 856.1 eV and 874.1 eV peaks of Ni 3+ The two strongly oscillating satellite peaks can also be attributed to indicate oxidation.

[0103] Fig.10 (c) is the high-resolution XPS spectrum of S 2p Through the fitting results, we can attribute the peak with a binding energy of 160.5 eV to S 2- while the two peaks at 162.5 eV and 161.9 eV can be attributed to S x- (2 < x < 8), where S is a partially reduced compound. The peak at 167.1 eV indicates oxidation caused by S.

[0104] Fig.10 (d) is the high-resolution XPS spectrum of O, which can be deconvoluted into three typical types of oxygen. The O1 peak can be attributed to the oxygen element combined with the metal, the O3 peak can be attributed to the hydroxyl species of the adsorbed water molecules on the surface, and the O2 peak can be attributed to the low-coordinated oxygen at the defective sites on the surface. According to the previous XRD results, we found that Ni and Co mainly combine with the S element. Therefore, the metal-oxygen bonds of O1 in XPS rarely match the XRD results. At the same time, the large appearance of O2 indicates that there are a large number of defective sites on the surface of the catalyst, and a large number of defective sites can provide additional conductive carriers, which can improve the conductivity of the catalyst to some extent.

[0105] 5. Electrochemical performance analysis of CoS-NiS / NCF

[0106] (1) HER performance analysis

[0107] All electrochemical tests were completed in a classical three-electrode system, and the electrolyte was 1.0 M KOH aqueous solution. The reference electrode used was a mercury oxide electrode, the counter electrode was a carbon rod, and the working electrode was a 0.5 cm X 0.5 cm sample.

[0108] In Fig.11 (a) Rare NCF, polarization curves of three different samples after foam sulfidation (NiS / NF, CoS / CF, CoS-NiS / NCF) and Pt / C sample. First, the overpotentials at small currents of 10 mA cm -2 and 100 mA cm -2 were evaluated. The overpotentials corresponding to Rare NCF, NiS / NF, CoS-NiS / NCF, and Pt / C at 10 mA cm -2211mV, 99mV, 59mV and 30mV, 10mA cm -2 The overpotentials at 1000 mA cm-1 were 345 mV, 224 mV, 186 mV and 120 mV. The CoS / CF sample could not read the parameters of the low current part due to the huge reduction peak. By comparison, it was found that CoS-NiS / NCF was the catalyst with the best potential at low current except for commercial Pt / C, especially compared with nickel-cobalt alloy foam. -2 The overpotentials of Rare NCF, NiS / NF, CoS / CF, and CoS-NiS / NCF under high current are 528mV, 387mV, 473mV, and 328mV, respectively. Pt / C cannot measure 1000mA cm -2 CoS-NiS / NCF has excellent performance under high current.

[0109] The Tafel slope is another performance index extrapolated from the polarization curve and can be used as an important parameter for judging the reaction dynamics. Fig.11 (b) is the Tafel slope of Rare NCF, NiS / NF, CoS / CF, CoS-NiS / NCF and Pt / C, where the Tafel slope of CoS-NiS / NCF is 49.4 mV dec. -1 Its value is much lower than 139.2mV dec of Rare NCF, NiS / NF, and CoS / CF samples. -1 , 110.1mV dec -1 , 89.6mV dec -1 It is worth noting that even compared with the 31.8 mV dec of the commercial catalyst Pt / C -1 Compared with the previous version, it still has certain advantages.

[0110] Fig.11 (c) is the electrochemical impedance spectroscopy of Rare NCF, NiS / NF, CoS / CF and CoS-NiS / NCF, where the Rct of the four samples is 28.2Ω, 12.36Ω, 3.15Ω and 0.77Ω. The smaller the Rct value, the faster the charge transfer rate, and the CoS-NiS / NCF value is 0.77Ω, which is excellent. Mass activity (MA) is the current per unit mass. Although it is not an evaluation of the intrinsic activity of the catalyst, it can be used as one of the reasonable parameters for evaluating the activity of the catalyst to a certain extent.

[0111] Fig.11 (d) The mass activities of NiS / NF, CoS / CF, CoS-NiS / NCF and Pt / C at 100 mV are 1.1 Ag, respectively. -1, 0.27A g -1 , 3.2A g -1 and 6.5A g -1 Although there is still a gap with commercial Pt / C, its value is far away from NiS / NF and CoS / CF, which shows that CoS-NiS / NCF has great activity per unit mass.

[0112] The conversion frequency can evaluate the number of catalytic reactions that occur on the active sites of the cobalt catalyst per unit time. This value can well illustrate the number of exposed active sites. Fig.11 (e) is the TOF graph of NiS / NF, CoS / CF, CoS-NiS / NCF and Pt / C. At 100 mV, the values ​​corresponding to NiS / NF, CoS / CF, CoS-NiS / NCF and Pt / C are 0.52S -1 , 0.12S -1 , 5.8S -1 and 7.8S -1 By comparison, we found that the TOF of CoS-NiS / NCF is very different from that of NiS / NF and CoS / CF, indicating that it has a large number of exposed active sites, while there is not much difference compared with commercial Pt / C, which further demonstrates the superiority of the catalytic activity of our catalyst.

[0113] In addition, we also compared it with recent related studies. Fig.11 (f) is a comparison of the Tafel slope and overpotential of the catalysts reported in the present invention and in recent literature, Fe-Ni3S2 / AF (59mV, 103mV dec -1 )(Wang M, Zhang L, Pan J, et al. A highly efficient Fe-doped Ni3S2electrocatalyst foroverall water splitting[J]. Nano Research, 2021, 14(12): 4740-4747), Fe 4.5 Ni 4.5 S8(179mV,83mV dec -1)(Piontek S,Andronescu C,Zaichenko A,et al.Influence of theFe:Ni Ratio and Reaction Temperature on the Efficiency of(Fex Ni1–x)9S8Electrocatalysts Applied in the Hydrogen Evolution Reaction[J].ACS Catalysis,2018,8(2):987-996)、(NiCo) 0.85 Se(169mV,115mV dec -1 )(Wu X,He D,Zhang H,etal.Ni0.85Se as an efficient non-noble bifunctional electrocatalyst for fullwater splitting[J].International Journal of Hydrogen Energy,2016,41(25):10688-10694)、C-S-FeNi / NF(85mV,93mV dec -1 )(Feng K,Song R,Xu J,et al.The S-Fe(Ni)sub-surface active sites for efficient and stable overall water splitting[J].Applied Catalysis B:Environmental,2023,325:122365)、MoOx / Ni3S2 / NF(106mV,90mV dec -1 )(Wu Y,Li G,Liu Y,et al.Overall Water Splitting CatalyzedEfficiently by an Ultrathin Nanosheet-Built,Hollow Ni3S2-BasedElectrocatalyst[J].Advanced Functional Materials,2016,26(27):4839-4847)、NiCo2S4(80mV,58mV dec -1)(Kang Z,Guo H,Wu J,et al.Engineering an Earth-AbundantElement-Based Bifunctional Electrocatalyst for Highly Efficient and DurableOverall Water Splitting[J].Advanced Functional Materials,2019,29(9):1807031)、Ni-Co-S / CF(140mV,96mV dec -1 )(Liu T,Sun X,Asiri AM,et al.One-step electrodeposition of Ni–Co–S nanosheets film as a bifunctional electrocatalyst for efficient water splitting[J]. dec -1 )(Yang Y,Yao H,Yu Z,et al.Hierarchical Nanoassembly of MoS2 / Co9S8 / Ni3S2 / Ni as aHighlyEfficient Electrocatalyst for Overall Water Splitting in a Wide pH Range[J].Journal of the American Chemical Society,2019,141(26):10417-10430 in NiTe-NiSe / NFF(76mV,61mV dec -1 )(Wang J,Huang J,Chen G,et al.In-situ engineered heterostructured nickel tellurium-selenide nanosheets for robust overall watersplitting[J].Chemical Engineering Journal,2022,446:137297), high voltage voltage (59mV,49.4mV dec -1 )Access to the snow-covered area.

[0114] (2) OER performance analysis

[0115] The OER test was also completed under a three-electrode system.

[0116] Fig.12 (a) is the polarization curves of five catalysts. The first comparison is the polarization curves of Rare NCF, CoS / CF, CoS-NiS / NCF and RuO2 (commercially available) at 10 mA cm -2 The overpotentials are 346 mA cm -2 , 83 mA cm -2 , 98 mA cm -2 and 235mA cm -2 By comparison, the catalytic performance of CoS-NiS / NCF is better than that of commercial RuO2, but slightly worse than that of CoS / NF at low current. NiS / NF cannot be compared due to the presence of oxidation peaks. We also selected 200mA cm -2 The overpotentials of Rare NCF, CoS / CF, NiS / NF, CoS-NiS / NCF and RuO2 are 502 mA cm -2 , 336 mA cm -2 , 376 mA cm -2 , 319 mA cm -2 and 340mA cm -2 As the current increases, our catalyst is still better than commercial RuO2 and CoS / CF. We also compared the 500mA cm -2 The overpotentials of Rare NCF, CoS / CF, NiS / NF, CoS-NiS / NCF and RuO2 are 544 mA cm -2 , 397 mA cm -2 , 445mA cm -2 , 371mA cm -2 and 398 mA cm -2 By comparison, we found that our CoS-NiS / NCF is still better than commercial RuO2. At the same time, our CoS-NiS / NCF can also reach 1000mA cm at 423mV. -2 The current density of commercial RuO2 cannot reach 1000mA cm -2 of current density.

[0117] Fig.12(b) is the Tafel slope of Rare NCF, CoS / CF, NiS / NF, CoS-NiS / NCF and RuO2. The values ​​of Rare NCF, CoS / CF, NiS / NF, CoS-NiS / NCF and RuO2 are 99.2 mV dec, respectively. -1 , 94.2mV dec -1 , 96.8mVdec -1 , 65.4mV dec -1 and 56.6mV dec -1 By comparing CoS-NiS / NCF’s 65.4mV dec -1 It is much better than Rare NCF, CoS / CF, NiS / NF, and the gap with RuO2 is very small, which means that the reaction kinetics of our CoS-NiS / NCF is very close to that of commercial RuO2. In order to evaluate the charge transfer rate in the reaction, we also tested the impedance of Rare NCF, CoS / CF, NiS / NF and CoS-NiS / NCF. The Rct of the four catalysts are 25.1Ω, 2.69Ω, 10.71Ω and 1.14Ω respectively. CoS-NiS / NCF has the lowest Rct, which means it has a very fast electron transfer rate.

[0118] In order to evaluate the sample unit mass current density, we also tested the mass activity of the samples. We compared the mass activities of CoS / CF, CoS-NiS / NCF and RuO2 at 300 mV, which were 6.2 A g -1 , 12.3A g -1 and 9.36A g -1 , where NiS / NF has no value because the oxidation peak cannot read the exact number, we take NiS / NF at 400mV 5.6A g -1 By comparison, it can be seen that the CoS-NiS / NCF catalyst has higher mass activity than RuO2.

[0119] Fig.12 (e) is the conversion frequency diagram of the catalyst, which is used to evaluate the intrinsic performance of the catalyst. The 300 mV value is taken as the evaluation value. The values ​​of NiS / NF, CoS / CF, CoS-NiS / NCF and RuO2 are 3.05S -1 , 2.92S -1 , 5.8S -1 and 6.45S -1 , among which CoS-NiS / NCF has a conversion frequency close to that of RuO2.

[0120] In addition, we also compared it with recently reported catalysts. Fig.12(f) is similar to the catalyst reported in the recent literature at 10 mA cm -2 Comparison of overpotential and Tafel slope at Mo-Co(OH)2(210mV,90mV dec -1 )(XuC, Lu W, Yan L, et al. Hierarchical molybdenum-doped cobaltous hydroxidenanotubes assembled by cross-linked porous nanosheets with efficientelectronic modulation toward overall water splitting[J]. Journal of Colloidand Interface Science, 2020,562:400-408), NiFe-MnCo2O4 / NFF(274mV,74mV dec -1 )(LinY,Yang Z,Cao D,et al.Electro-deposition of nickel–iron nanoparticles onflower-like MnCo2O4 nanowires as an efficient bifunctional electrocatalyst for overall water splitting[J].CrystEngComm,2020,22(8):1425-1435),Ni3S2 / NF(136mV,102mV dec -1 )(Wu Y, Li G, Liu Y, et al. Overall Water Splitting CatalyzedEfficiently by an Ultrathin Nanosheet-Built, Hollow Ni3S2-BasedElectrocatalyst[J]. Advanced Functional Materials, 2016, 26(27): 4839-4847), Ni-Co-S / CF (247mV, 109mV dec -1)(Liu T,Sun X,Asiri AM,et al.One-stepelectrodeposition of Ni–Co–S nanosheets film as a bifunctionalelectrocatalyst for efficient water splitting[J].International Journal ofHydrogen Energy,2016,41(18):7264-7269)、Ni-250-2@NF(289mV,95mV dec -1 )(Wang S,Zhang Y,Deng X,et al.Rational construction of loosely packed nickelnanoparticulates with residual HCOO ligands derived from a Ni-MOF for high-efficiency electrocatalytic overall water splitting[J].Journal of MaterialsChemistry A,2023,11(10):5222-5232)、Cu3Se2@CoSe2-NiSe2 / PNCF(240mV,87mV dec -1 )(Wang G,Huang J,Chen G,et al.In-Situ-Engineered 3D Cu3 Se2@CoSe2–NiSe2Nanostructures for Highly Efficient Electrocatalytic Water Splitting[J].ACSSustainable Chemistry&Engineering,2020,8(46):17215-17224)、N-NiVFFeP / NFF(229mV,72mV dec -1)(Fan H, Chen W, Chen G, et al. Plasma-heteroatom-doped Ni-V-Fetrimetallic phospho-nitride as high-performance bifunctional electrocatalyst [J]. Applied Catalysis B: Environmental, 2020, 268: 118440), NCS / NS-rGo (322mV, 81mVdec -1 )(Li H, Chen L, Jin P, et al. NiCo2S4 microspheres grown on N,S co-dopedreduced graphene oxide as an efficient bifunctional electrocatalyst foroverall water splitting in alkaline and neutral pH [J]. Nano Research, 2022, 15 (2): 950-958) and NiTe-NiSe / NFF (164mV, 53mV dec -1 )(Wang J, Huang J, Chen G, et al. In-situ engineered heterostructured nickel tellur-selenide nanosheets for robust overall water splitting[J]. Chemical Engineering Journal, 2022, 446: 137297), by comparison, it was found that the CoS-NiS / NCF catalyst of the present invention has a 98mV, 65mV dec -1 There is considerable competition among the recently reported catalysts.

[0121] (3) Electrochemical surface area analysis

[0122] Electrochemical surface area (ECSA) can be used to compare the electrochemically active surface area of ​​catalysts. It can be calculated using the formula ECSA = C dl / Cs(Cs=0.04mF cm -2 ), where Cdl is the double layer capacitance. From the formula, we can see that ECSA and C dl It is a proportional relationship, so we can compare the corresponding C dl To compare the size of ECSA.

[0123] Fig.13 (b), (d) and (f) are the corresponding C of NiCo alloy foam, Ni foam and Co foam after vulcanization. dl The corresponding slope of the fitting curve is half of C. dl Value, among which the C of nickel-cobalt alloy foam dl Maximum 22.0mF cm -2 The worst nickel foam is 2.7mF cm -2 , Co foam is 16.5mF cm -2 Therefore, it can be concluded that the sample corresponding to the nickel-cobalt alloy foam is used for a larger ECSA, which is consistent with the morphology results in the SEM, further illustrating that the unique morphology of the needle-shaped leaves can increase the specific surface area of ​​the catalyst, thereby achieving a lower overpotential when the same current density is achieved.

[0124] (4) HER and OER stability analysis

[0125] In addition to the excellent catalytic activity of the catalyst, the long-term electrolysis stability of the catalyst is also an important parameter for evaluating the catalyst performance. Fig.14 It is a stability test of the catalyst, which is evaluated from two aspects.

[0126] First, the polarization curves of the catalysts before 10,000 CV cycles were compared. Fig.14 (a) and (b) are the LSV comparisons of HER and OER before 10,000 CV cycles. It is not difficult to find that even after 10,000 CV cycles, the performance of HER and OER has not been greatly reduced, and they still have excellent low-current and high-current performance. In addition, we also conducted long-term HER and OER electrolysis tests on the catalyst at constant potential.

[0127] Fig.14 (c) is the result of the stability test of HER at a current density of 100 mA cm-250 h under the given initial potential. After 50 h of long-term electrolysis, the current density of the catalyst increased by 6%.

[0128] After the HER test, we conducted a long-term electrolysis test on the same sample at 200mA cm-2 for 50h. Fig.14 As shown in (d), the current density only decreases by 3%, which also proves that our catalyst has good electrocatalytic stability.

[0129] In summary, the catalyst prepared by the present invention has a highly efficient HER and OER dual-functional electrocatalytic material, and has higher stability and greater current density than the catalysts in the prior art.

[0130] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a CoS-NiS / NCF catalyst, characterized in that: The following steps are involved: S1. Clean the NiCo foam and dry it for later use; S2, mixing ammonium fluoride, urea and S powder with deionized water, and then stirring the mixed solution for a period of time, and then performing ultrasonic treatment; S3, placing the NiCo foam in step S1 and the mixed solution in step S2 into a reactor to react for a period of time; S4. After the reaction is completed, the NiCo foam is taken out, cleaned and dried to obtain the CoS-NiS / NCF catalyst.

2. The method for preparing a CoS-NiS / NCF catalyst according to claim 1, characterized in that: Step S1 specifically includes: The NiCo foam was placed in an acetone solution and subjected to ultrasonic treatment; after the ultrasonic treatment, the acetone on the surface of the NiCo foam was cleaned with ethanol and deionized water respectively; then the NiCo foam was placed in an HCl solution and subjected to ultrasonic treatment; after the ultrasonic treatment, the acetone on the surface of the NiCo foam was cleaned with ethanol and deionized water respectively, and the solution was dried for later use.

3. The method for preparing a CoS-NiS / NCF catalyst according to claim 2, characterized in that: In step S1, the power of the two ultrasonic treatments is 50-70 W, and the ultrasonic time is 8-12 min.

4. The method for preparing a CoS-NiS / NCF catalyst according to claim 1, characterized in that: In step S2, the mass ratio of ammonium fluoride, urea and S powder is 200-250:450-500:58-98.

5. The method for preparing a CoS-NiS / NCF catalyst according to claim 1, characterized in that: In step S2, the mixed solution is stirred at a rotation speed of 800 to 1200 rpm for 8 to 12 minutes.

6. The method for preparing a CoS-NiS / NCF catalyst according to claim 1, characterized in that: In step S2, ultrasound is performed at a power of 80 to 120 W for 8 to 12 minutes.

7. The method for preparing a CoS-NiS / NCF catalyst according to claim 1, characterized in that: In step S3, the reaction is carried out at a temperature of 140 to 170° C. for 4 to 9 hours.

8. The method for preparing a CoS-NiS / NCF catalyst according to claim 1, characterized in that: In step S4, the NiCo foam is dried at 40-60° C. for 1.5-2.5 h.

9. A CoS-NiS / NCF catalyst obtained by the method according to any one of claims 1 to 8.

10. Use of the CoS-NiS / NCF catalyst as claimed in claim 9 in hydrogen production.

Citation Information

Patent Citations

  • Nano-rod array composite material as well as preparation method and application thereof

    CN108816250A

  • NiFe(CN)5NO-Ni3S2-NF composite catalyst prepared by two-step solvothermal method and application of NiFe(CN)5NO-Ni3S2-NF composite catalyst

    CN113026049A

  • Cobalt-nickel metal sulfide bifunctional electrocatalyst as well as preparation method and application thereof

    CN115029709A

  • Preparation method and application of NiCo-like hydrotalcite / Ni3S2 / Co9S8 composite nanosheet electrode material

    CN116334681A

  • Molybdenum oxide-nickel sulfide heterostructure nano array electrocatalyst and preparation method thereof

    CN116516401A

Cited By

  • Nickel-based chalcogenide catalyst as well as preparation method and application thereof

    CN121853033A