Device and method for machining diamond roller through line anode rotary scanning electro-deposition
By using line anode rotating scanning electrodeposition technology, combined with nickel sulfamate solution and multiple line anode rotating scanning devices, the problems of low current density and weak coating holding force in traditional electrodeposition methods have been solved, and efficient and dense diamond roller electrodeposition layers have been prepared.
Patent Information
- Application Number
- CN202410942614.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional electrodeposition methods have low current density on diamond rollers, resulting in low deposition efficiency and weak holding force.
The linear anode rotating scanning electrodeposition technology is adopted, using nickel sulfamate solution. Through two steps of pre-plating and thickening plating, combined with multiple linear anode rotating scanning devices, the current density is increased and the density and holding power of the coating are enhanced.
It significantly improves the generation efficiency and density of diamond roller electrodeposition layers, while enhancing the adhesion between the coating and the diamond.
Smart Images

Figure CN118996589A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of diamond roller electrodeposition, and in particular relates to a device and a method for processing a diamond roller by using a wire anode rotary scanning electrodeposition. Background Art
[0002] Diamond rollers are now widely used in various places, such as manufacturing, construction, medical equipment, gemstones and jewelry. This is because diamond is one of the hardest materials in nature, which makes diamond rollers have excellent wear resistance and long life. In the field of high-precision processing, diamond rollers play an important role. The electroplating process for diamond roller production now generally adopts a nickel sulfate electroplating process with nickel sulfate as the main salt or an aminosulfonic acid nickel electroplating process with nickel aminosulfonic acid as the main salt. The characteristics of the nickel sulfate electroplating process are fine crystallization and good density of the coating. However, the allowable current density is low and the electroplating cycle is long. In addition, due to the presence of sodium chloride in the nickel sulfate electroplating solution, the internal stress of the coating is large, and there are quality risks of blistering and shelling of the coating for large diamond rollers. The characteristics of the aminosulfonic acid nickel electroplating process are fast deposition speed, low stress and high flatness of the prepared nickel layer. For example, the patent application number CN113564643A discloses the use of NiSO 4 The method of layered electrodeposition using nickel sulfamate solution is that the deposited layer is denser when nickel sulfate solution is used for electrodeposition, but the deposition efficiency is lower. The nickel sulfamate solution allows a larger current density and a higher deposition efficiency, but the density of the deposited layer and the coating holding force are weaker.
[0003] Line anode rotary scanning electrodeposition is a unique electrodeposition processing method. It realizes electrodeposition by rotating and scanning a linear anode close to the cathode. Therefore, the electroplated layer obtained by the method of line anode scanning electrodeposition processing diamond roller can reach nanometer scale, and the coating holding force is strong. At the same time, the line anode can provide a higher current density, and the deposition efficiency of the line scanning electrodeposition electroplated layer is higher. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for rapidly preparing a diamond roller electrodeposition layer with excellent holding force of the electrodeposition layer.
[0005] The purpose of the present invention is to overcome the drawbacks of traditional electrodeposition methods, such as the low current density provided by the traditional electroplated diamond roller anode, resulting in low efficiency in deposited layer generation and weak holding force of the deposited layer, and thus provide a unique scanning electrodeposition processing device and method.
[0006] The specific operation steps are as follows: place the female mold on the bracket in the plating tank, place the wire anode component in the middle of the female mold, use nickel sulfamate solution as the electroplating solution, first perform the pre-plating electro-deposition step, and then perform the thickening plating step. Make the coating thickness meet the process requirements. This method uses multiple wire anode rotating scanning devices for diamond roller electro-deposition technology, which can greatly improve the efficiency of electro-deposition processing, and the nickel plating structure is more dense, while ensuring the hardness of the diamond roller coating, it also improves the holding force between the coating and the diamond.
[0007] A device and method for machining a diamond roller by wire anode rotary scanning electrodeposition comprises the following steps:
[0008] Step 1, preparation before plating:
[0009] The negative mold is used as the electroplating cathode and connected to the negative pole of the power supply. The anode platinum sheet of the electroplating tank is connected to the positive pole of the power supply. The negative mold is placed on the bottom frame of the electroplating tank. The electroplating solution is a nickel sulfamate solution, including components and mass concentrations of Ni(NH 2 SO 3 ) 2 ·4H 2 O 500g / L; H 3 BO 3 30g / L.
[0010] Step 2, electroplating:
[0011] First, a pre-plating is performed with a current density of 1.1-2A / dm 2 The electroplating time is 0.5h to complete the pre-plating step. The current density is 0.01-0.02A / (dm 2 ·min) to stabilize the current density at 2-7A / dm 2 , and conduct secondary electroplating for 8-10 days. After completing the electroplating thickening step, a negative mold with a complete coating is obtained. The electroplating solution is a nickel sulfamate solution.
[0012] In the step 1, the female mold is sanded in advance.
[0013] In step 1, only 20-50 um width of the anode platinum sheet is exposed.
[0014] In the step 1, the number of anodes in the electroplating device line is 1-6.
[0015] In the step 2, electroplating is performed once, the electroplating temperature is 40-55° C., and the pH value of the plating solution is 4.0-4.5.
[0016] In the step 2, the secondary electroplating is performed, the electroplating temperature is 40-70° C., and the pH value of the plating solution is 3.5-4.5.
[0017] In the step 2, after the secondary electroplating, the thickness of the nickel plating layer is 2.0-2.5 mm.
[0018] In the step 2, the line anode scanning speed is 40-80 mm / s.
[0019] In the step 2, the female mold with nickel plating is used for subsequent processing of the diamond roller.
[0020] In the step 2, the prepared coating has a microhardness of 480-500 HV and an internal stress of 3.24-4.92 MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 A schematic diagram of a device and method for machining a diamond roller by using a wire anode rotary scanning electrodeposition method implemented by the present invention;
[0022] Figure 2 A top view of a device and method for machining a diamond roller by using a wire anode rotary scanning electrodeposition according to the present invention;
[0023] The reference numerals in the figure are: 1-anode cavity, 2-anode platinum sheet, 3-female mold, 4-base, 5-anode support, 6-plating tank, 7-liquid outlet, 8-slip ring, 9-anode wire; DETAILED DESCRIPTION
[0024] The present invention is further described in detail below with reference to examples.
[0025] The nickel sulfamate plating solution used in the following examples includes components and a mass concentration of Ni(NH 2 SO 3 ) 2 ·4H 2 O500g / L; H 3 BO 3 30g / L.
[0026] Example 1
[0027] A device and method for machining a diamond roller by wire anode rotary scanning electrodeposition, comprising the following steps:
[0028] Step 1, preparation before plating:
[0029] Schematic diagram of nickel plating on the negative mold of the diamond roller carrier Figure 1As shown, the electroplating device structure includes an anode cavity 1, an anode platinum sheet 2, a female mold 3, a base frame 4, an anode bracket 5, and a plating tank 6. The female mold is fixed on the base frame and connected to the power supply. The female mold is connected to the cathode of the power supply, and four wire anode cavities and platinum sheets are connected to the anode of the power supply. The platinum sheet is 100 mm long, 10 mm wide, and 50 μm thick. It is embedded in the anode cavity to expose a linear anode with a length of 100 mm and a thickness of 50 μm, which is polished flat. After the female mold is sanded, it is placed in the electroplating tank liquid. According to the different stages of pre-plating and thickening plating, different current densities are provided in sections to make the inner cavity surface of the female mold fit tightly with the nickel plating layer of diamond, and the diamond layer is firmly held on the inner cavity surface of the female mold. The operation is terminated after the plating reaches a certain thickness. The subsequent specific steps are as follows:
[0030] Step 2, electroplating;
[0031] First, a pre-plating was performed, the plating temperature was 40°C, the plating solution pH was 4.0, and the current density was 1.1A / dm 2 The line scanning speed was 40 mm / s and the electroplating time was 0.5 h to complete the pre-plating step. The current density was 0.01 A / (dm 2 ·min) to stabilize the current density at 4A / dm 2 The thickening plating step was carried out, the electroplating temperature was 50° C., the pH value of the plating solution was 3.5, the line anode scanning speed was 50 mm / s, the electroplating time was 8 d, and the plating solution was a nickel sulfamate solution.
[0032] After the electroplating process is completed, the coating thickness is 2.2mm, and a negative mold with a nickel coating is obtained. The microhardness of the coating is tested to be 488.6HV, and the internal stress is 3.46MPa, which is used for subsequent processing of diamond rollers.
[0033] Example 2
[0034] A device and method for machining a diamond roller by wire anode rotary scanning electrodeposition, comprising the following steps:
[0035] Step 1, preparation before plating:
[0036] Schematic diagram of carrier negative mold electroplating for processing diamond rollers Figure 1As shown, the electroplating device structure includes an anode cavity 1, an anode platinum sheet 2, a female mold 3, a base frame 4, an anode bracket 5, and a plating tank 6. The female mold is fixed on the base frame and connected to the power supply. The female mold is connected to the cathode of the power supply, and four wire anode cavities and platinum sheets are connected to the anode of the power supply. The platinum sheet is 100 mm long, 10 mm wide, and 50 μm thick. It is embedded in the anode cavity to expose a linear anode with a length of 100 mm and a thickness of 50 μm, which is polished flat. After the female mold is sanded, it is placed in the electroplating tank liquid. According to the different stages of pre-plating and thickening plating, different current densities are provided in sections to make the inner cavity surface of the female mold fit tightly with the nickel plating layer of diamond, and the diamond layer is firmly held on the inner cavity surface of the female mold. The operation is terminated after the plating reaches a certain thickness. The subsequent specific steps are as follows:
[0037] Step 2, electroplating
[0038] First, a pre-plating was performed, the plating temperature was 42°C, the plating solution pH was 4.0, and the current density was 1.2A / dm 2 The line scanning speed was 45 mm / s and the electroplating time was 0.5 h to complete the pre-plating step. The current density was 0.01 A / (dm 2 ·min) was increased, and the current density was finally stabilized at 4.2A / dm 2 The thickening plating step was performed, the electroplating temperature was 55° C., the plating solution pH was 3.5, the line anode scanning speed was 55 mm / s, the electroplating time was 8 d, and the plating solution was a nickel sulfamate solution.
[0039] After the electroplating process is completed, the coating thickness is 2.5mm, and a negative mold with a nickel coating is obtained. The microhardness of the coating is tested to be 485HV and the internal stress is 3.7MPa, which is used for subsequent processing of diamond rollers.
[0040] Example 3
[0041] A device and method for machining a diamond roller by wire anode rotary scanning electrodeposition, comprising the following steps:
[0042] Step 1, preparation before plating:
[0043] Schematic diagram of carrier negative mold electroplating for processing diamond rollers Figure 1As shown, the electroplating device structure includes an anode cavity 1, an anode platinum sheet 2, a female mold 3, a base frame 4, an anode bracket 5, and a plating tank 6. The female mold is fixed on the base frame and connected to the power supply. The female mold is connected to the cathode of the power supply, and three wire anode cavities and platinum sheets are connected to the anode of the power supply. The platinum sheet is 100 mm long, 10 mm wide, and 50 μm thick. It is embedded in the anode cavity to expose a linear anode with a length of 100 mm and a thickness of 50 μm, which is polished flat. After the female mold is sanded, it is placed in the electroplating tank liquid. According to the different stages of pre-plating and thickening plating, different current densities are provided in sections to make the inner cavity surface of the female mold fit tightly with the diamond nickel plating layer, and the diamond layer is firmly held on the inner cavity surface of the female mold. The operation is terminated after the plating reaches a certain thickness. The subsequent specific steps are as follows:
[0044] Step 2, electroplating:
[0045] First, a pre-plating was performed, the plating temperature was 45°C, the plating solution pH was 4.0, and the current density was 1.5A / dm 2 The line scanning speed was 48 mm / s and the electroplating time was 0.5 h to complete the pre-plating step. The current density was 0.01 A / (dm 2 ·min) to stabilize the current density at 3A / dm 2 The thickening plating step was carried out, the electroplating temperature was 60°C, the pH of the plating solution was 3.5, the line anode scanning speed was 40 mm / s, the electroplating time was 8 days, and the plating solution was a nickel sulfamate solution.
[0046] After the electroplating process is completed, the coating thickness is 2mm, and a negative mold with a nickel coating is obtained. The microhardness of the coating is tested to be 498HV and the internal stress is 3MPa, which is used for subsequent processing of diamond rollers.
[0047] Example 4
[0048] A device and method for machining a diamond roller by wire anode rotary scanning electrodeposition, comprising the following steps:
[0049] Step 1, preparation before plating:
[0050] Schematic diagram of carrier negative mold electroplating for processing diamond rollers Figure 1As shown, the electroplating device structure includes an anode cavity 1, an anode platinum sheet 2, a female mold 3, a base frame 4, an anode bracket 5, and a plating tank 6. The female mold is fixed on the base frame and connected to the power supply. The female mold is connected to the cathode of the power supply, and three wire anode cavities and platinum sheets are connected to the anode of the power supply. The platinum sheet is 100 mm long, 10 mm wide, and 50 μm thick. It is embedded in the anode cavity to expose a linear anode with a length of 100 mm and a thickness of 50 μm, which is polished flat. After the female mold is sanded, it is placed in the electroplating tank liquid. According to the different stages of pre-plating and thickening plating, different current densities are provided in sections to make the inner cavity surface of the female mold fit tightly with the diamond nickel plating layer, and the diamond layer is firmly held on the inner cavity surface of the female mold. The operation is terminated after the plating reaches a certain thickness. The subsequent specific steps are as follows:
[0051] Step 2, electroplating:
[0052] First, a pre-plating was performed, the plating temperature was 40°C, the plating solution pH was 4.0, and the current density was 1.5A / dm 2 The line scanning speed was 45 mm / s and the electroplating time was 0.5 h to complete the pre-plating step. The current density was 0.01 A / (dm 2 ·min) to stabilize the current density at 2.5A / dm 2 The thickening plating step was carried out, the electroplating temperature was 50°C, the pH of the plating solution was 3.5, the line anode scanning speed was 55 mm / s, the electroplating time was 8 days, and the plating solution was a nickel sulfamate solution.
[0053] After the electroplating process is completed, the coating thickness is 1.8mm, and a negative mold with a nickel coating is obtained. The microhardness of the coating is tested to be 483HV, and the internal stress is 3.23MPa, which is used for subsequent processing of diamond rollers.
Claims
1. A device and method for machining a diamond roller by wire anode rotary scanning electrodeposition, characterized in that: It includes the following steps: Step 1: Preparation before plating: The electroplating system device is installed and debugged, and the anode platinum sheet (2) is embedded in the anode cavity (1), and the anode platinum sheet is exposed only by 20-50um, so that it forms a linear anode scanning structural component, and the female mold is detachably installed horizontally on the base frame (4), and the surface of the linear anode structure platinum sheet and the surface of the female mold are separated by a constant gap, and the female mold is used as the electroplating cathode and connected to the negative electrode of the power supply. After the anode in the electroplating tank is connected to the positive electrode of the power supply, the female mold is placed in the plating solution of the electroplating tank; wherein, the anode is introduced into the technology of preparing diamond roller by linear anode high current density scanning electroplating, and the plating solution in the electroplating tank flows out from the hole (8); Step 2: Electroplating: First, pre-plating is performed to plate a thin nickel layer on the roller substrate with a current density of 1.1-2A / dm 2 After the pre-plating step is completed, the current density is then increased to 0.01-0.02A / (dm 2 ·min) to stabilize the current density at 2-7A / dm 2 , a thickening plating step is performed, and after the electrodeposition thickening plating step is completed, a negative mold with a complete plating layer is obtained.
2. The device and method for machining a diamond roller by wire anode rotary scanning electrodeposition according to claim 1, characterized in that: In the step 1, the anode of the electrodeposition system device adopts a linear anode rotation scanning method.
3. The device and method for machining a diamond roller by wire anode rotary scanning electrodeposition according to claim 1, characterized in that: In the step 1, the linear anode is a platinum sheet with a purity of 99.99%, a length of 80-110 mm, a width of 5-20 mm, and a thickness of 20-50 μm. The sheet is embedded in organic glass to expose the linear anode, and then polished to be flat.
4. The device and method for machining a diamond roller by wire anode rotary scanning electrodeposition according to claim 1, characterized in that: In the step 2, the line anode scanning speed is 40-80 mm / s.
5. The device and method for machining a diamond roller by wire anode rotary scanning electrodeposition according to claim 1, characterized in that: In step 2, after the thickening plating step, the thickness of the nickel plating layer is 2.0-2.5 mm.
6. The device and method for machining a diamond roller by wire anode rotary scanning electrodeposition according to claim 1, characterized in that: In step 2, the gap between the surface of the wire anode platinum sheet and the surface of the cathode is 100-500um.
7. The device and method for machining a diamond roller by wire anode rotary scanning electrodeposition according to claim 1, characterized in that: In the step 1, the number of anodes in the electroplating device line is 1-6.
Citation Information
Cited By
Archimedes spiral anode rotary scanning electroforming device
CN121321110A