Soft PVC artificial leather with low plasticizer content

By reducing the amount of plasticizer in PVC artificial leather and combining other ingredients to modify, the PU swelling and material brittle cracking caused by plasticizer migration in traditional PVC artificial leather is solved, reducing environmental and health risks and prolonging product life cycles and maintains the flexibility and physical properties of the material.

CN118996866APending Publication Date: 2024-11-22CANADIAN GENERAL TOWER CHANGSHU CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411303611.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The high content of traditional PVC artificial leather plasticizers leads to deterioration of the mechanical properties of the material, increased greasiness on the surface, environmental pollution and health risks, especially in high temperature environments, which leads to swelling of PU artificial leather and brittle cracking of the material, affecting service life and appearance quality. .

Method used

Using soft PVC artificial leather structure with low plasticizer content, including surface treatment layer, PVC dense layer, PVC foam layer, PVC glue layer and base cloth layer, it is modified by reducing the amount of plasticizer and combining with other ingredients. Reduce the environmental and health threat of plasticizers while maintaining the flexibility and physical properties of the material.

Benefits of technology

It significantly reduces the plasticizer content, extends the life cycle of PVC artificial leather, reduces dependence on traditional plasticizers, reduces environmental and health risks, maintains the soft feel and physical properties of the material, and broadens the scope of application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118996866A_ABST
    Figure CN118996866A_ABST
Patent Text Reader

Abstract

The invention discloses soft PVC artificial leather with low plasticizer content. The soft PVC artificial leather comprises a surface treatment layer, a PVC compact layer, a PVC foaming layer, a PVC glue layer and a base cloth layer from top to bottom, the PVC compact layer comprises the following components in parts by weight: 70 parts of PVC resin, 40-50 parts of a phthalate plasticizer, 5-40 parts of PNBR powder nitrile rubber, 5-15 parts of CPE chlorinated polyethylene, 5-15 parts of a propenyl elastomer and 16 parts of other functional aids. According to the invention, the problem of PU artificial leather swelling caused by plasticizer precipitation during contact application of PVC and PU can be solved, the problem of embrittlement caused by plasticizer loss due to long-term application of a PVC artificial leather material is further solved, the product life cycle of the PVC artificial leather is prolonged, and meanwhile, the harm of the plasticizer to the environment and the health of passengers is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of automobile interior decoration materials, in particular to a soft PVC artificial leather with low plasticizer content. Background Art

[0002] Among automotive interior materials, PVC (polyvinyl chloride) artificial leather is widely used due to its excellent durability, plasticity and economy. However, in order to meet the stringent flexibility and feel requirements of automotive interior materials, traditional PVC formulas usually contain a high proportion of plasticizers, usually reaching 40% to 50% of the weight of PVC in the formula. The role of plasticizers is to lower the glass transition temperature of PVC, making it softer and improving its processability.

[0003] Commonly used plasticizers include phthalates (such as DPHP) and nonyl esters. Although these plasticizers can effectively improve the flexibility and feel of PVC, their migration during use will cause a series of problems, such as decreased mechanical properties of the material, increased surface greasiness, and pollution to the vehicle interior environment. Especially in the field of automotive interiors, long-term exposure to high temperature environments will cause more serious volatilization and migration of plasticizers, resulting in:

[0004] 1. Induce PU leather to swell: When PVC and PU leather are used together in car interiors, due to the long-term contact between PVC and PU materials, the plasticizer in the PVC leather migrates to the surface and then penetrates into the PU leather in contact with it, eventually causing the PU leather to swell. The essence of this is that after the plasticizer penetrates into the PU, its polar groups rob the hydrogen bonds between the PU molecular chains, causing changes in the PU molecular structure.

[0005] 2. Material brittle cracking: With the migration and volatilization of plasticizers, the plasticizer content inside PVC decreases. When it reaches the limit, the flexibility and physical properties of the material will drop sharply, resulting in cracks on the surface of the material, which will ultimately affect the service life and appearance quality of the car interior.

[0006] 3. Environmental and health impacts of plasticizers: Especially phthalate plasticizers, which may have potential environmental and health risks. Some phthalate plasticizers are considered to have potential reproductive toxicity and are subject to increasingly stringent regulations. Summary of the invention

[0007] The purpose of the present invention is to provide a soft PVC artificial leather with a low plasticizer content, which can improve the quality and service life of the PVC artificial leather by reducing the amount of plasticizer used, while reducing the threat of plasticizer to the environment and passenger health.

[0008] To this end, the present invention provides the following technical solution:

[0009] A soft PVC artificial leather with low plasticizer content, comprising: from top to bottom, a surface treatment layer, a PVC dense layer, a PVC foaming layer, a PVC glue layer, and a base fabric layer;

[0010] The PVC dense layer comprises the following components:

[0011] 70 parts of PVC resin,

[0012] Phthalate plasticizer 40-50 parts,

[0013] PNBR powder nitrile rubber 5-40 parts,

[0014] CPE chlorinated polyethylene 5-15 parts,

[0015] 5-15 parts of propylene-based elastomer,

[0016] 16 parts of other functional additives.

[0017] Preferably, the PVC foam layer is added with 0.5 parts of foaming agent on the basis of the PVC dense layer.

[0018] Preferably, the other functional additives include 5 parts of filler, 5 parts of stabilizer, 5 parts of masterbatch, 0.5 parts of compatibilizer and 0.5 parts of lubricant.

[0019] Preferably, the PVC resin is a calendering grade PVC resin with a degree of polymerization of 700-1300.

[0020] Preferably, the phthalate plasticizer is one or more of diisononyl phthalate, dibutyl phthalate, diisobutyl phthalate or diphenyl phthalate.

[0021] Preferably, the PNBR powdered nitrile rubber is a powdered nitrile rubber having an acrylonitrile content of 28-38%.

[0022] Preferably, the CPE chlorinated polyethylene is chlorinated polyethylene having a chlorine content of 34-44%.

[0023] Preferably, the propylene-based elastomer is a propylene-ethylene copolymer having a Shore A hardness in the range of 50-70A.

[0024] In order to solve the above technical problems, the present invention also provides a method for preparing the PVC artificial leather, comprising the steps of:

[0025] Step 1: Apply PVC glue on the surface of the base fabric layer by gravure printing, plasticize at 160-200℃, and wait for post-processing;

[0026] Step 2: by calendering, add the above prepared PVC dense layer formula raw materials and 0.5 weight parts of foaming agent in an internal mixer for melt blending, then successively pass through a double-roll open mill, filter through an extruder, and press through a four-roller to obtain a foaming layer film with uniform thickness, and then pass through a composite roller to composite the obtained foaming layer film with the base fabric with PVC glue in step 1, and after passing through a cooling roller, wait for post-processing;

[0027] Step 3: melt and blend the raw materials of the dense layer in proportion in an internal mixer by calendaring, then successively pass through a double-roll open mixer, filter through an extruder, and thin through a four-roll press to obtain a dense layer film with uniform thickness, and then pass through a composite roller to composite the obtained PVC dense layer film with the semi-finished product in step 2, and after passing through a cooling roller, wait for post-processing;

[0028] Step 4: Send the semi-finished product in step 3 to the foaming production line, foam it at a high temperature of 200-230°C in the foaming furnace, and wait for post-processing;

[0029] Step 5: coating the artificial leather semi-finished product foamed in step 4 with a surface treatment agent, and subjecting it to a high-temperature embossing treatment at 160° C. to obtain the PVC artificial leather.

[0030] The beneficial effects of the present invention are:

[0031] (1) The soft PVC artificial leather with low plasticizer content of the present invention solves the problem of PU artificial leather swelling caused by plasticizer precipitation when PVC and PU are in contact and applied by reducing the plasticizer content and combining with other components for blending and modification, thereby broadening the scope of product application, and further solving the problem of brittle cracking caused by plasticizer loss in long-term application of PVC artificial leather materials, thereby extending the product life cycle of PVC artificial leather; through blending and modification, the flexibility of PVC artificial leather materials mainly depends on the elastic properties of the copolymer itself, thereby reducing the dependence on traditional plasticizers. Compared with traditional high-plasticizer PVC formulas, this method can significantly reduce the plasticizer content while maintaining the physical properties of the material. The amount of plasticizer used is reduced, and the hardening problem caused by plasticizer loss is greatly reduced. PVC artificial leather will be able to maintain a consistent soft feel throughout its life cycle.

[0032] (2) The PVC artificial leather of the present invention reduces the amount of the speed increasing agent, thereby reducing the potential threat of the plasticizer to the environment and the health of passengers, and reduces the harmful substances released when the PVC artificial leather is exposed to a high temperature environment for a long time.

[0033] (3) In the preparation of the PVC artificial leather of the present invention, although in order to reduce the plasticizer content, a blending modification method is used to add different weight portions of components to the dense layer, the introduction of the copolymer does not require major adjustments to the existing processing equipment and processes. The existing processing equipment and processes are still applicable, that is, they are suitable for the existing PVC processing flow, thereby reducing the cost and time of process improvement. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a cross-sectional schematic diagram of a soft PVC artificial leather with low plasticizer content of the present invention;

[0035] Figure 2 This is a schematic diagram of the different pattern retention levels of the control PVC artificial leather used in the test after 7 days of heat aging at 120 degrees;

[0036] Figure 3 It is a schematic diagram of the swelling change level of the control PU surface used in the test. DETAILED DESCRIPTION

[0037] The preferred embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0038] Embodiment 1:

[0039] This embodiment introduces a method for preparing soft PVC artificial leather with low plasticizer content.

[0040] like Figure 1 As shown, Figure 1 The cross-sectional schematic diagram of a soft PVC artificial leather with low plasticizer content of the present invention. A soft PVC artificial leather with low plasticizer content comprises: from top to bottom, a surface treatment layer, a PVC dense layer, a PVC foaming layer, a PVC glue layer, and a base fabric layer;

[0041] The PVC dense layer comprises the following components:

[0042] 70 parts of PVC resin,

[0043] Phthalate plasticizer 50 parts,

[0044] PNBR powder nitrile rubber 30 parts,

[0045] CPE chlorinated polyethylene 10 parts,

[0046] 15 parts of propylene elastomer,

[0047] 16 parts of other functional additives.

[0048] Wherein, the other functional additives include 5 parts of filler, 5 parts of stabilizer, 5 parts of masterbatch, 0.5 parts of compatibilizer and 0.5 parts of lubricant.

[0049] The dense layer formula is shown in Table 1.

[0050]

[0051] The only difference between the foam layer and the dense layer formula is whether a foaming agent is added.

[0052] In this embodiment, the PVC foaming layer is added with 0.5 parts of foaming agent on the basis of the PVC dense layer. The PVC resin is a calendering grade PVC resin with a polymerization degree of 700-1300.

[0053] The phthalate plasticizer is one or more of diisononyl phthalate, dibutyl phthalate, diisobutyl phthalate or diphenyl phthalate.

[0054] The PNBR powdered nitrile rubber is a powdered nitrile rubber with an acrylonitrile content of 28-38%.

[0055] The chlorinated polyethylene is a chlorinated polyethylene with a chlorine content of 34-44%.

[0056] The propylene-based elastomer is a propylene-ethylene copolymer with a Shore A hardness in the range of 50-70A, and the propylene-based elastomer is ExxonMobil-Vistamax.

[0057] The other functional additives include fillers, stabilizers, masterbatches, compatibilizers, and lubricants.

[0058] Wherein, the foaming agent is a commercially available azodicarbonamide foaming agent.

[0059] The glue layer is a commercially available general high-temperature resistant hot melt adhesive, and the base fabric layer is a commercially available general knitted fabric, preferably a four-way stretch base fabric, with a thickness of 0.6-0.8 cm.

[0060] The artificial leather semi-finished product is prepared by the above PVC dense layer ratio. The PVC foaming layer formula is only based on the PVC dense layer formula, and 0.5 parts by weight of foaming agent is added. The detailed preparation method is as follows:

[0061] Step 1: Apply commercially available PVC glue on the surface of the base fabric layer by gravure printing, plasticize at 200 degrees, and wait for post-processing;

[0062] Step 2: by calendering, add the above prepared PVC dense layer formula raw materials and 0.5 parts by weight of foaming agent into an internal mixer for melt blending, then successively pass through a double-roll open mill, filter through an extruder, and press through a four-roll mill to obtain a foaming layer film with uniform thickness, and then pass through a composite roller to composite the obtained foaming layer film with the base fabric layer with PVC glue in step 1, and after passing through a cooling roller, wait for post-processing;

[0063] Step 3: by calendering, add the above proportioned PVC dense layer formula raw materials into an internal mixer for melt blending, then successively pass through a double-roll open mill, filter through an extruder, and thin through a four-roll press to obtain a dense layer film with uniform thickness, and then pass through a composite roller to composite the obtained PVC dense layer film with the semi-finished product in step 2, and after passing through a cooling roller, wait for post-processing;

[0064] Step 4: Send the semi-finished product in step 3 to the foaming production line, foam it in a foaming furnace at 220 degrees for 1 minute, and wait for post-processing;

[0065] Step 5: coating the artificial leather semi-finished product foamed in step 4 with a surface treatment agent, and embossing at a high temperature of 160° C. to obtain the PVC artificial leather.

[0066] The surface treatment agent used in the surface treatment layer is a commercially available general PVC artificial leather treatment agent.

[0067] Example 2

[0068] The soft PVC artificial leather with low plasticizer content of the present invention was prepared in the same manner as in Example 1, except that the composition ratio of the PVC dense layer was as shown in Table 2.

[0069]

[0070] Example 3

[0071] The soft PVC artificial leather with low plasticizer content of the present invention was prepared in the same manner as in Example 1, except that the composition ratio of the PVC dense layer was as shown in Table 3.

[0072]

[0073]

[0074] Example 4

[0075] The soft PVC artificial leather with low plasticizer content of the present invention was prepared in the same manner as in Example 1, except that the composition ratio of the PVC dense layer was as shown in Table 4.

[0076]

[0077] Example 5

[0078] The soft PVC artificial leather with low plasticizer content of the present invention was prepared in the same manner as in Example 1, except that the composition ratio of the PVC dense layer was as shown in Table 5.

[0079]

[0080] Comparative Example 1

[0081] The soft PVC artificial leather with low plasticizer content of the present invention was prepared in the same manner as in Example 1, except that the composition ratio of the PVC dense layer was as shown in Table 6.

[0082]

[0083]

[0084] Comparative Example 2

[0085] The soft PVC artificial leather with low plasticizer content of the present invention was prepared in the same manner as in Example 1, except that the composition ratio of the PVC dense layer was as shown in Table 7.

[0086]

[0087] Comparative Example 3

[0088] The soft PVC artificial leather with low plasticizer content of the present invention was prepared in the same manner as in Example 1, except that the composition ratio of the PVC dense layer was as shown in Table 8.

[0089]

[0090] Comparative Example 4

[0091] The soft PVC artificial leather with low plasticizer content of the present invention was prepared in the same manner as in Example 1, except that the composition ratio of the PVC dense layer was as shown in Table 9.

[0092]

[0093] Comparative Example 5

[0094] The soft PVC artificial leather with low plasticizer content of the present invention was prepared in the same manner as in Example 1, except that the composition ratio of the PVC dense layer was as shown in Table 10.

[0095]

[0096] Performance testing and evaluation were carried out through the above Examples 1-5 and Comparative Examples 1-5:

[0097] 1. After 7 days of heat aging at 120 degrees, observe the pattern retention rate. Figure 2 As shown, Figure 2 This is a schematic diagram of the different pattern retention levels of the control PVC artificial leather used in the test after 7 days of heat aging at 120 degrees. Figure 2 As a basis for rating, by comparing with the heat aging grade of the control PVC artificial leather, the pattern retention rate of Examples 1-5 and Comparative Examples 1-5 after heat aging was observed, and the test personnel visually compared the pattern changes under a 20x magnifying glass and rated them. The evaluation results are shown in Table 11.

[0098] 2. Rigidity and softness evaluation

[0099] According to the GMW 3390 method, the stiffness and softness test is carried out. The larger the test value, the higher the hardness. The standard requires that the stiffness and softness range of PVC artificial leather should be 60-100mm.

[0100] 3.PU swelling

[0101] The products in the above-mentioned Examples 1-5 and Comparative Examples 1-5 were cut into the same size and placed on the surface of the PU artificial leather, wherein the PVC was on the top and the PU was on the bottom, and the PVC artificial leather surface was in contact with the PU artificial leather surface, ensuring that the PVC and PU were in full contact.

[0102] There is no phenomenon of warping, etc. Place the above samples in an 80-degree oven and let them stand for 48 hours. Observe the changes on the PU surface and rate the samples, with the highest being level 5. Rating reference Figure 3 As shown, Figure 3 This is a schematic diagram of the swelling change level of the control PU surface used in the test. Figure 3 As the basis for rating, the rating results are shown in Table 11.

[0103] 4. Evaluation of bending resistance

[0104] At room temperature, the products in the above embodiments and comparative examples are cut into the same size and placed on a folding endurance tester for testing. The tests are performed 10,000 times, 50,000 times, 100,000 times, 150,000 times and 200,000 times, respectively, and the highest number of times the sample can pass is recorded (if it passes the bending test of 130,000 times but fails the 150,000 times, it is recorded as 100,000 times).

[0105] Table 11 Performance test results of the embodiments and comparative examples

[0106]

[0107] The test shows that the artificial leather obtained from Examples 1-5 has excellent hand feel, soft material, good pattern retention, no swelling phenomenon occurs when in contact with PU, and the bending resistance after high-temperature aging can always meet the automotive spec requirements and meet the expected requirements.

[0108] Compared with Example 1, the amount of propylene-based elastomer in Comparative Example 1 is increased, and relatively speaking, the content of PVC resin and plasticizer is decreased, the overall rigidity of the material is decreased, and the temperature resistance is decreased, which ultimately leads to the disappearance of the pattern after high temperature.

[0109] Compared with Example 1, since the temperature resistance of the propylene-based elastomer is poor, as the content of the propylene-based elastomer decreases, although the pattern is slightly improved after high temperature, the bending resistance of the material is significantly attenuated.

[0110] Compared with Example 1, Comparative Example 3 reduces the use of CPE raw materials. Since the CPE material itself has excellent temperature resistance, as the amount used decreases, the temperature resistance decreases. After 7 days of heat aging at 120 degrees, the pattern of the material becomes significantly lighter, which is not enough to meet the requirements for automotive use.

[0111] Compared with Example 1, Comparative Example 4 removes the PNBR component in the formula. PNBR has excellent resilience and makes a great contribution to the elasticity and flexibility of the artificial leather. As its dosage decreases, the rigidity of the material increases significantly.

[0112] Compared with Example 1, the amount of plasticizer used in Comparative Example 5 is significantly increased. With the large amount of plasticizer used, plasticizer migration is inevitable after long-term high temperature, which ultimately leads to swelling of the PU artificial leather in contact with it and a decrease in its bending resistance.

[0113] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A soft PVC artificial leather with low plasticizer content, characterized in that: include: From top to bottom, it includes surface treatment layer, PVC dense layer, PVC foam layer, PVC glue layer, and base fabric layer; The PVC dense layer comprises the following components: PVC resin 70 parts, Phthalate plasticizer 40-50 parts, PNBR powder nitrile rubber 5-40 parts, CPE chlorinated polyethylene 5-15 parts, 5-15 parts of propylene-based elastomer, 16 parts of other functional additives.

2. The soft PVC artificial leather with low plasticizer content according to claim 1, characterized in that: The PVC foaming layer is added with 0.5 parts of foaming agent on the basis of the PVC dense layer.

3. The soft PVC artificial leather with low plasticizer content according to claim 1, characterized in that: The other functional additives include 5 parts of filler, 5 parts of stabilizer, 5 parts of masterbatch, 0.5 parts of compatibilizer and 0.5 parts of lubricant.

4. The soft PVC artificial leather with low plasticizer content according to claim 1, characterized in that: The PVC resin is a calendering grade PVC resin with a polymerization degree of 700-1300.

5. The soft PVC artificial leather with low plasticizer content according to claim 1, characterized in that: The phthalate plasticizer is one or more of diisononyl phthalate, dibutyl phthalate, diisobutyl phthalate or diphenyl phthalate.

6. The soft PVC artificial leather with low plasticizer content according to claim 1, characterized in that: The PNBR powdered nitrile rubber is a powdered nitrile rubber with an acrylonitrile content of 28-38%.

7. The soft PVC artificial leather with low plasticizer content according to claim 1, characterized in that: The CPE chlorinated polyethylene is chlorinated polyethylene with a chlorine content of 34-44%.

8. The soft PVC artificial leather with low plasticizer content according to claim 1, characterized in that: The propylene-based elastomer is a propylene-ethylene copolymer with a Shore A hardness in the range of 50-70A.

9. The method for preparing a soft PVC artificial leather with low plasticizer content according to claims 1-8, characterized in that: Includes steps: Step 1: Apply PVC glue on the surface of the base fabric layer by gravure printing, plasticize at 160-200℃, and wait for post-processing; Step 2: by calendering, add the above prepared PVC dense layer formula raw materials and 0.5 parts by weight of foaming agent into an internal mixer for melt blending, then successively pass through a double-roll open mill, filter through an extruder, and press through a four-roll mill to obtain a foaming layer film with uniform thickness, and then pass through a composite roller to composite the obtained foaming layer film with the base fabric layer with PVC glue in step 1, and after passing through a cooling roller, wait for post-processing; Step 3: melt and blend the raw materials of the PVC dense layer in proportion in an internal mixer by calendaring, then successively pass through a double-roll open mixer, filter through an extruder, and thin through a four-roll press to obtain a dense layer film with uniform thickness, and then pass through a composite roller to composite the obtained PVC dense layer film with the semi-finished product in step 2, and after passing through a cooling roller, wait for post-processing; Step 4: Send the semi-finished product in step 3 to the foaming production line, foam it at a high temperature of 200-230°C in a foaming furnace, and wait for post-processing; Step 5: coating the artificial leather semi-finished product foamed in step 4 with a surface treatment agent, and subjecting it to a high-temperature embossing treatment at 160° C. to obtain the PVC artificial leather.