Method for preparing antibacterial anti-aging paper-based material from polyphenol modified fibroin fiber composite bamboo pulp
Through the composite treatment of polyphenol-modified silk fiber and bamboo pulp, the problems of low strength and easy aging of paper-based materials are solved, and the antibacterial aging resistance is improved, and it is suitable for specific packaging materials.
Patent Information
- Application Number
- CN202411250306.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-22
AI Technical Summary
Existing paper-based materials have low strength, are prone to aging and lack antibacterial properties. In particular, bamboo pulp paper loses antibacterial components during the preparation process and cannot effectively inhibit bacterial growth.
Method for preparing antibacterial and aging-resistant paper-based materials using polyphenol-modified silk fiber composite bamboo pulp. By treating silk fibers with polyphenol-metal complexing solution and combining them with bamboo pulp, paper-based materials with antibacterial and antioxidant properties are formed. Material. The method includes degumming, beating and washing the silk fibers, mixing them with bamboo pulp and baking to prepare a paper-based material with enhanced strength and antibacterial properties.
It improves the strength performance of paper-based materials and gives them antibacterial and aging resistance, can effectively inhibit the growth of bacteria such as Staphylococcus aureus and E. coli, is suitable for food and drug packaging, and shows significant durability in aging tests.
Smart Images

Figure BDA0005032056210000101 
Figure BDA0005032056210000111 
Figure BDA0005032056210000112
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of functional material processing, and in particular to a method for preparing an antibacterial and aging-resistant paper-based material by using polyphenol-modified silk fibroin fiber composite bamboo pulp. Background Art
[0002] Tea polyphenols have strong antioxidant effects, especially the ester-type catechin epigallocatechin gallate (EGCG), whose reducing ability can even reach 100 times that of L-isoascorbic acid. Among the four main catechin compounds, the antioxidant capacity is epigallocatechin gallate (EGCG) > epigallocatechin (EGC) > epicatechin gallate (ECG) > epicatechin (EC), and the antioxidant performance increases with the increase of temperature. In addition to its antioxidant effect, tea polyphenols also have antibacterial effects, such as inhibiting Staphylococcus, Escherichia coli, Candida albicans, Bacillus subtilis, etc.
[0003] The fiber structure of silk is very similar to that of plant fibers. The beating characteristics of silk fibers are similar to those of plant fibers, and both have fibrillation characteristics. Therefore, it can be used in the papermaking industry after being processed by pulping and papermaking processes. Silk has good biocompatibility, biodegradability, air permeability, moisture permeability, slow release properties and excellent mechanical properties, which are advantages that plant fibers do not have. At the same time, natural silk fibers have well-organized intermediate structures, including microfibers, nanofibers and nanoparticles. These mesoscale structures are usually well organized into complex arrangements and, as part of natural silk fibers, have strong mechanical properties and functions. Silk fibers are stripped into different mesoporous structures, including microfibers, nanofibers, nanorods and nanoparticles. Based on these mesoporous silks, they have the advantages of adjustable size, clear size distribution, high modulus, good redispersibility and good processability. At the same time, the rich fibril structure after the silk fiber splitting treatment significantly increases the exposed hydroxyl and amino groups in the fiber after the splitting, providing a structural basis for the modification of the fiber. However, most of the existing silk degumming technologies are alkaline degumming, with a temperature of 90-100°C, using sodium bicarbonate and sodium carbonate, which has the problem of incomplete degumming, and the use of sodium hydroxide, which damages the silk fibroin, causes high pollution and high energy consumption. In addition, as a natural protein fiber, silk still has many shortcomings. For example, silk has poor UV resistance and is prone to yellowing and aging when exposed to sunlight for a long time.
[0004] During the preparation process of bamboo pulp paper, the antibacterial component bamboo Kun in bamboo fibers is almost completely removed. Therefore, ordinary bamboo pulp paper does not have antibacterial properties. Existing functional paper-based materials with antibacterial effects basically achieve the antibacterial effect by soaking in antibacterial liquid or setting an antibacterial layer. Therefore, it is extremely urgent to develop a paper material that can inhibit bacterial growth for a long time. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the present invention provides a method for preparing an antibacterial and aging-resistant paper-based material from polyphenol-modified silk fibroin fiber composite bamboo pulp. The antibacterial and aging-resistant paper-based material prepared by the method provided by the present invention has improved strength performance and at the same time has antibacterial and aging-resistant properties, effectively solving the problems of low strength, easy aging and ineffective antibacterial of existing paper-based materials.
[0006] To achieve the above-mentioned purpose, the technical solution adopted by the present invention to solve the technical problem is: to provide a method for preparing an antibacterial and aging-resistant paper-based material by using polyphenol-modified silk fibroin fiber composite bamboo pulp, comprising the following steps:
[0007] S1, adding water to the composite enzyme preparation and stirring evenly, adding raw silkworm cocoons, stirring and then discharging the waste liquid to obtain degummed silk fibroin fibers;
[0008] S2, washing the degummed silk fiber obtained in step S1, cutting it into small pieces, adding water to beat the pieces, filtering the water to obtain the fiberized silk fiber, and then adding the fiberized silk fiber into the polyphenol-metal complex solution and stirring it, and then extracting alkali coordination after sufficient penetration to obtain the polyphenol-metal modified silk fiber;
[0009] S3, washing the polyphenol-metal modified silk fiber obtained in step S2 with deionized water, and then adding bamboo pulp board and water for pulping to obtain slurry;
[0010] S4, adding sizing agent and water to the slurry obtained in step S3, mixing and then sequentially performing sheet making, roller pressing and drying to obtain an antibacterial and aging-resistant paper-based material.
[0011] Further, in step S1, the complex enzyme preparation includes the following components in parts by weight: 2-4 parts of papain, 1-3 parts of trypsin, 1-2 parts of pectinase, 2-4 parts of disodium hydrogen phosphate and 1-2 parts of sodium dihydrogen phosphate.
[0012] Furthermore, the preparation method of the above-mentioned complex enzyme preparation comprises the following steps: fully mixing papain, trypsin, pectinase, disodium hydrogen phosphate and sodium dihydrogen phosphate.
[0013] Furthermore, in step S1, the mass ratio of the complex enzyme preparation, raw silkworm cocoons and water is 1-2:250-350:9500-10500.
[0014] Further, in step S1, the pH value is 8-10, the temperature is 45-55° C., and the stirring is performed at 60-80 r / min. The stirring time is 4-6 minutes, and the stirring time is stopped for 9-11 minutes. This process is repeated 6-8 times.
[0015] Further, in step S2, washing is performed with deionized water.
[0016] Furthermore, in step S2, the mass ratio of the deionized water used for washing to the raw silkworm cocoons in step S1 is 3:10.
[0017] Further, in step S2, the mixture is stirred at 60-80 r / min for 4-6 min, then drained and washed 3-5 times.
[0018] Further, in step S2, the pieces are cut into small segments with a length of 1-3 cm.
[0019] Furthermore, in step S2, the mass ratio of the degummed silk fibroin fibers to the water used for pulping is 1:100.
[0020] Further, in step S2, the beating degree is 20-30.
[0021] The beneficial effect of adopting the above further scheme is that the silk fibers are split and peeled into different mesoporous structures and more polar groups are exposed.
[0022] Furthermore, in step S2, the mass ratio of the silk fibroin fibers to the polyphenol-metal complex solution after fiber division is 1-2:18-22.
[0023] Furthermore, in step S2, the method for preparing the polyphenol-metal complex solution comprises the following steps: adding polyphenol and metal salt into a citric acid solution, and stirring the mixture sufficiently at room temperature to obtain a polyphenol-metal complex solution.
[0024] Furthermore, the polyphenol is at least one of epicatechin, epigallocatechin, epicatechin gallate and epigallocatechin gallate.
[0025] Furthermore, the metal salt is at least one of aluminum salt, calcium salt, zinc salt, silver salt and titanium salt.
[0026] Further, the pH value of the citric acid solution is 2-3.
[0027] Furthermore, the mass ratio of polyphenol to citric acid solution is 1-4:100.
[0028] Furthermore, in the polyphenol-metal complex solution, the molar concentration of metal ions is 0.1-1 mol / L.
[0029] Further, in step S2, stirring is performed at 35-50°C and 60-80r / min, stirring for 4-6min each time, stopping for 9-11min, repeating 6-8 times, and then adjusting the pH value to 5-7, continuing stirring at a speed of 60-80r / min, stirring for 4-6min each time, stopping for 9-11min, repeating 2-4 times and then draining the liquid.
[0030] Furthermore, the pH value was adjusted to 5-7 using sodium hydroxide at a concentration of 1 mol / L.
[0031] Furthermore, in step S3, the mass ratio of the polyphenol-metal modified silk fiber to the deionized water used for washing is 2-4:9-11.
[0032] Furthermore, in step S3, the mass ratio of the polyphenol-metal modified silk fiber to the deionized water used for washing is 3:10.
[0033] Further, in step S3, the mixture is stirred at a speed of 60-80 r / min for 4-6 min, then drained and washed 3-5 times.
[0034] Furthermore, in step S3, the mass ratio of the polyphenol-metal modified silk fiber, the bamboo pulp board and the water used for pulping is 7-8:2-3:100.
[0035] Further, in step S4, the mass ratio of the sizing agent, water and the slurry obtained in step S3 is 2-4:1800-2200:90-110.
[0036] Furthermore, in step S4, the sizing agent is at least one of gelatin, starch, polyvinyl alcohol and carboxymethyl cellulose.
[0037] The antibacterial and aging-resistant paper-based material is prepared by the method for preparing the antibacterial and aging-resistant paper-based material by using the polyphenol-modified silk fibroin fiber composite bamboo pulp.
[0038] The present invention has the following beneficial effects:
[0039] 1. The present invention is based on the structural basis of polyphenolic substances and the performance basis of anti-oxidation and antibacterial, combined with the structural characteristics of rich active groups such as carboxyl and amino groups on the silk protein peptide chain, using metal ions as bridges, forming a polyphenol-metal-silk protein framework through metal ion coordination, enhancing the stability of silk fiber, while retaining the air permeability and softness of silk fiber, giving silk fiber antibacterial and antioxidant properties, and the modified silk fiber can be applied to paper-based composite materials. The antibacterial and aging-resistant paper-based material prepared by the method provided by the present invention has greatly improved strength performance under the premise of meeting national standards, and has both antibacterial and aging-resistant properties, and can be applied to specific food and drug packaging.
[0040] 2. The present invention utilizes the principle that the active group phenolic hydroxyl in the structure of catechin polyphenols can form coordination bonds with metal ions, and the active group carboxyl of silk fibroin can also form coordination bonds with metal ions. Metal ions are used as bridges to form coordination bonds with polyphenols and proteins at the same time. At the same time, the number of coordination bonds changes with the change of pH value. Suitable metal ions are matched, and the pH value is accurately controlled. The number of coordination bonds at low pH values is small, which promotes material penetration. The alkali is then extracted to promote coordination and complexation, and a polyphenol-metal-protein spatial structure is constructed. The stability of the protein is improved, the mechanical strength is increased, and the polyphenol also has antioxidant and antibacterial properties. It is compounded with bamboo pulp to prepare paper-based materials, and the strength performance of the obtained paper-based materials meets national standards; the obtained paper is compared with ordinary paper through aging tests, and the aging resistance of the paper of the present invention is improved. Using the antibacterial zone experiment to detect, the obtained paper has an inhibitory effect on Staphylococcus aureus, Escherichia coli, and Bacillus subtilis.
[0041] 3. The present invention selects sodium dihydrogen phosphate and disodium hydrogen phosphate as buffers, which can phosphorylate the hydroxyl groups on the serine or tyrosine side chains in the enzyme molecules, thereby forming a reversible covalent modification. At the same time, pectinase, papain, and trypsin are used to configure the composite enzyme preparation. Each single enzyme in the composite enzyme preparation has enzyme catalytic specificity and can specifically degrade organic matter. At the same time, the end product of the multi-enzyme system acts as an inhibitor to bind to the allosteric site of the key enzyme and quickly adjust the function of the active center of the enzyme, thereby achieving the effect of quickly adjusting the entire metabolic pathway. The composite enzyme preparation can achieve a degumming rate of 30% under the conditions of a temperature of 30-50°C and a pH value of 7.5-9.5. The composite enzyme method is used for degumming, and the degumming effect is good. The morphology of the silk fiber is complete. The degumming rate at a temperature of 35-50°C reaches 30%. The use of the biological enzyme method for degumming has low energy consumption, good waste liquid degradability, and high environmental protection. DETAILED DESCRIPTION
[0042] The principles and features of the present invention are described below, and the examples are only used to explain the present invention and are not used to limit the scope of the present invention. If no specific conditions are specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0043] Example 1
[0044] The method for preparing antibacterial and aging-resistant paper-based material by using polyphenol-modified silk fiber composite bamboo pulp comprises the following steps:
[0045] S1, adding water to the composite enzyme preparation and stirring evenly, adding raw silkworm cocoons, stirring at a speed of 70r / min under the conditions of pH 9 and temperature of 50°C, stirring for 5 minutes each time, stopping for 10 minutes, repeating 7 times, and then discharging the waste liquid to obtain degummed silk fibroin fibers, wherein the composite enzyme preparation comprises the following components in parts by weight: 3 parts of papain, 2 parts of trypsin, 1 part of pectinase, 3 parts of disodium hydrogen phosphate and 1 part of sodium dihydrogen phosphate, and the mass ratio of the composite enzyme preparation, raw silkworm cocoons and water is 1:300:10000;
[0046] S2, washing the degummed silk fiber obtained in step S1 with deionized water, stirring at a speed of 70r / min for 5min and then draining, repeating the washing 4 times, and then shearing into small segments of 1-3cm and beating with water, wherein the mass ratio of the degummed silk fiber to the beating water is 1:100, the beating degree is 25, filtering the water and dividing the silk fiber, adding epicatechin gallate and aluminum chloride to a citric acid solution with a pH value of 2, and fully stirring at room temperature to obtain an epicatechin gallate-aluminum complex solution, wherein the molar concentration of aluminum ions is 0.5mol / L, and the mass ratio of epicatechin gallate to the citric acid solution is 3:100, Then, the fiberized silk fibers are added to the epicatechin gallate-aluminum complex solution and stirred at a speed of 70 r / min at 40° C. The stirring is repeated for 7 times with a stirring time of 5 min and a stop time of 10 min. The pH value is adjusted to 6 using sodium hydroxide having a concentration of 1 mol / L. The fibers are then stirred at a speed of 70 r / min. The stirring is repeated for 3 times with a stirring time of 5 min and a stop time of 10 min. The liquid is then drained to obtain polyphenol-metal modified silk fibers. The mass ratio of the deionized water used for washing to the raw silk cocoons in step S1 is 3:10, and the mass ratio of the fiberized silk fibers to the epicatechin gallate-aluminum complex solution is 1:20.
[0047] S3, washing the polyphenol-metal modified silk fiber obtained in step S2 with deionized water, stirring at a speed of 70 r / min for 5 min and then draining, repeating the washing 4 times, and then adding a bamboo pulp board and water for beating to obtain a slurry, wherein the mass ratio of the polyphenol-metal modified silk fiber to the deionized water used for washing is 3:10, and the mass ratio of the polyphenol-metal modified silk fiber, the bamboo pulp board and the water used for beating is 7:2:100;
[0048] S4. Add gelatin and water to the slurry obtained in step S3, mix well, and then successively perform sheet making, roller pressing and drying to obtain an antibacterial and aging-resistant paper-based material. The mass ratio of the gelatin, water and the slurry obtained in step S3 is 3:2000:100.
[0049] Example 2
[0050] The method for preparing antibacterial and aging-resistant paper-based material by using polyphenol-modified silk fiber composite bamboo pulp comprises the following steps:
[0051] S1, dissolving the composite enzyme preparation in water, adding raw silkworm cocoons, stirring at a speed of 60r / min under the conditions of pH 8 and temperature of 45°C, stirring for 4min each time, stopping for 9min, repeating 6 times, and then discharging the waste liquid to obtain degummed silk fibroin fibers, wherein the composite enzyme preparation comprises the following components in parts by weight: 2 parts of papain, 1 part of trypsin, 1 part of pectinase, 2 parts of disodium hydrogen phosphate and 1 part of sodium dihydrogen phosphate, and the mass ratio of the composite enzyme preparation, raw silkworm cocoons and water is 1:250:9500;
[0052] S2, the degummed silk fiber obtained in step S1 is washed with deionized water, stirred at a speed of 60r / min for 4min and then drained, and the washing is repeated 3 times, and then sheared into small segments of 1-3cm and then beaten with water, the mass ratio of the degummed silk fiber to the beating water is 1:100, the beating degree is 20, the water is filtered and the silk fiber is divided into fibers, epigallocatechin gallate, epigallocatechin, epicatechin gallate, aluminum chloride, zinc sulfate and calcium chloride are added to a citric acid buffer solution with a pH value of 3, and fully stirred at room temperature to obtain epigallocatechin gallate-epigallocatechin-epicatechin gallate-aluminum-zinc-calcium complex solution, wherein the molar concentration of aluminum ions is 0.3mol / L, the molar concentration of zinc ions is 0.2mol / L, the molar concentration of calcium ions is 0.2mol / L, the molar concentration of epigallocatechin gallate, epigallocatechin, epicatechin gallate, aluminum chloride, zinc sulfate and calcium chloride are added to a citric acid buffer solution with a pH value of 3, and the solution is fully stirred at room temperature to obtain an epigallocatechin gallate-epigallocatechin-epicatechin gallate-aluminum-zinc-calcium complex solution, wherein the molar concentration of aluminum ions is 0.3mol / L, the molar concentration of zinc ions is 0.2mol / L, the molar concentration of calcium ions is 0.2mol / L, the molar concentration of epigallocatechin gallate, epigallocatechin The mass ratio of epigallocatechin gallate, epicatechin gallate and citric acid buffer is 1:1:1:100, and then the fiberized silk fiber is added to the epigallocatechin gallate-epicatechin gallate-epicatechin gallate-aluminum-zinc-calcium complex solution, and stirred at a speed of 60r / min at 35°C, stirring for 4min each time, stopping for 9min, repeating 6 times, adjusting the pH value to 5 with 1mol / L sodium hydroxide, and then continuing to stir at a speed of 60r / min, stirring for 4min each time, stopping for 9min, repeating 2 times, and then draining to obtain polyphenol-metal modified silk fiber, the mass ratio of the above-mentioned deionized water for washing to the raw silk cocoon in step S1 is 2:9, and the mass ratio of the above-mentioned silk fiber to the epigallocatechin gallate-epicatechin gallate-epicatechin gallate-aluminum-zinc-calcium complex solution is 1:18;
[0053] S3, washing the polyphenol-metal modified silk fiber obtained in step S2 with deionized water, stirring at a speed of 60 r / min for 5 min and then draining, repeating the washing 4 times, and then adding bamboo pulp board and water for beating to obtain slurry, wherein the mass ratio of the polyphenol-metal modified silk fiber to the deionized water used for washing is 2:9, and the mass ratio of the polyphenol-metal modified silk fiber, bamboo pulp board and water used for beating is 7:2:100;
[0054] S4. Add gelatin, sodium carboxymethyl cellulose, polyvinyl alcohol and water to the slurry obtained in step S3, mix well, and then successively carry out sheet making, roller pressing and drying to obtain an antibacterial and aging-resistant paper-based material. The mass ratio of the above gelatin, sodium carboxymethyl cellulose, polyvinyl alcohol, water and the slurry obtained in step S3 is 1:1:1:1800:90.
[0055] Example 3
[0056] The method for preparing antibacterial and aging-resistant paper-based material by using polyphenol-modified silk fiber composite bamboo pulp comprises the following steps:
[0057] S1, adding water to the composite enzyme preparation and stirring evenly, adding raw silk cocoons, stirring at a speed of 80r / min under the conditions of pH 10 and temperature of 55°C, stirring for 6 minutes each time, stopping for 11 minutes, repeating 8 times, and then discharging the waste liquid to obtain degummed silk fibroin fibers, wherein the composite enzyme preparation comprises the following components in parts by weight: 4 parts of papain, 3 parts of trypsin, 2 parts of pectinase, 4 parts of disodium hydrogen phosphate and 2 parts of sodium dihydrogen phosphate, and the mass ratio of the composite enzyme preparation, raw silk cocoons and water is 2:350:10500;
[0058] S2, washing the degummed silk fiber obtained in step S1 with deionized water, stirring at a speed of 80r / min for 6min and then draining, repeating the washing 5 times, and then shearing into small segments of 1-3cm and beating with water, wherein the mass ratio of the degummed silk fiber to the beating water is 1:100, the beating degree is 30, filtering the water and dividing the silk fiber, adding epigallocatechin and silver nitrate to a citric acid solution with a pH value of 3, and fully stirring at room temperature to obtain an epigallocatechin-silver nitrate complex solution, wherein the molar concentration of silver ions is 0.8mol / L, and the mass ratio of epicatechin gallate to the citric acid solution is 4:100, and then The fiberized silk fibers were added to the epigallocatechin-silver nitrate complex solution and stirred at 80 r / min at 50° C. The stirring was repeated for 6 min and 11 min, and the pH value was adjusted to 6.8 using 1 mol / L sodium hydroxide. The fibers were then stirred at 80 r / min and the stirring was repeated for 6 min and 11 min, and the solution was drained after 4 times to obtain polyphenol-metal modified silk fibers. The mass ratio of the deionized water used for washing to the raw silk cocoons in step S1 was 4:11, and the mass ratio of the fiberized silk fibers to the epigallocatechin-silver nitrate complex solution was 2:22.
[0059] S3, washing the polyphenol-metal modified silk fiber obtained in step S2 with deionized water, stirring at a speed of 80 r / min for 6 min and then draining, repeating the washing 5 times, and then adding bamboo pulp board and water for beating to obtain slurry, wherein the mass ratio of the polyphenol-metal modified silk fiber to the deionized water used for washing is 3:10, and the mass ratio of the polyphenol-metal modified silk fiber, bamboo pulp board and water used for beating is 8:3:100;
[0060] S4. Add polyvinyl alcohol and water to the slurry obtained in step S3, mix well, and then successively perform sheet making, roller pressing and drying to obtain an antibacterial and aging-resistant paper-based material. The mass ratio of the polyvinyl alcohol, water and the slurry obtained in step S3 is 4:2200:110.
[0061] Comparative Example 1
[0062] A method for preparing bamboo pulp paper comprises the following steps:
[0063] S1, adding bamboo pulp board into water, breaking it up and beating it to obtain wet pulp, wherein the mass ratio of bamboo pulp board to water is 1:100;
[0064] S2, uniformly mixing gelatin, polyvinyl alcohol, sodium carboxymethyl cellulose and water, and adding the mixture to the wet slurry obtained in step S1, and uniformly mixing to obtain a treated slurry, wherein the weight ratio of gelatin, polyvinyl alcohol, sodium carboxymethyl cellulose, water and the wet slurry obtained in step S1 is 1:1:1:100:100;
[0065] S3, the treated pulp obtained in step S2 is sheeted, rolled, dehydrated and dried on a papermaking machine to obtain bamboo pulp paper.
[0066] Comparative Example 2
[0067] A method for preparing polyphenol-bamboo pulp comprises the following steps:
[0068] S1, adding bamboo pulp board into water, breaking it up and beating it to obtain wet pulp, wherein the mass ratio of bamboo pulp board to water is 1:100;
[0069] S2, adding epigallocatechin gallate, epigallocatechin, epicatechin gallate and epicatechin to the wet slurry obtained in step S1, stirring at a speed of 60 r / min, stirring for 5 min and stopping for 10 min, repeating 6 times, and letting it stand for 2 h to obtain a mixed slurry, wherein the mass ratio of epigallocatechin gallate, epigallocatechin, epicatechin gallate and epicatechin to the wet slurry obtained in step S1 is 1:1:1:1:100;
[0070] S3, uniformly mixing gelatin, polyvinyl alcohol, sodium carboxymethyl cellulose and water, adding the mixture to the mixed slurry obtained in step S2, and uniformly mixing to obtain a treated slurry, wherein the weight ratio of gelatin, polyvinyl alcohol, sodium carboxymethyl cellulose, water and the mixed slurry obtained in step S2 is 1:1:1:100:100;
[0071] S4, the treated pulp obtained in step S3 is sheeted, rolled, dehydrated and dried on a paper machine to obtain polyphenol-bamboo pulp paper.
[0072] Test Example 1 Physical Test
[0073] The physical properties of the antibacterial and aging-resistant paper-based materials prepared in Examples 1-2, the bamboo pulp paper prepared in Comparative Example 1, and the polyphenol-bamboo pulp paper-based materials prepared in Comparative Example 2 were tested using a weathering instrument, and the test results of thickness, basis weight, folding endurance, tear resistance, and tensile strength are shown in Table 1.
[0074] Table 1 Physical properties test results of different materials
[0075]
[0076]
[0077] As can be seen from Table 1, when polyphenol-metal-silk fiber is applied to paper-based materials, the tensile strength, folding resistance, tear resistance, etc. of the paper-based materials are greatly improved, and the aging test is carried out using a weathering instrument. The polyphenol-metal-silk fiber paper-based material has both aging resistance and good aging performance.
[0078] Test Example 2 Antibacterial Activity Test
[0079] The antibacterial test was carried out according to GB T 20944.2-2007 Evaluation of antibacterial properties of textiles Part 3 Oscillation method standard. The results are shown in Table 2.
[0080] Table 2 Antibacterial test
[0081]
[0082]
[0083] As shown in Table 2, ordinary bamboo pulp paper does not have antibacterial properties. When polyphenols are added during the pulp preparation process, the antibacterial properties of the paper are improved, but the polyphenols are not firmly combined with the bamboo pulp, the residual amount is small, and the antibacterial properties are relatively weak. Through the method provided by the present invention, polyphenol-metal-silk fiber is combined through coordination bonds, hydrogen bonds and physical effects, and the obtained paper-based material has an antibacterial rate of more than 99% against Staphylococcus aureus, Escherichia coli and Candida albicans, and has good antibacterial properties.
[0084] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing antibacterial and aging-resistant paper-based materials by using polyphenol-modified silk fiber composite bamboo pulp, characterized in that: The following steps are involved: S1, adding water to the composite enzyme preparation and stirring evenly, adding raw silkworm cocoons, stirring and then discharging the waste liquid to obtain degummed silk fibroin fibers; S2, washing the degummed silk fiber obtained in step S1, cutting it into small pieces, adding water to beat the pieces, filtering the water to obtain the fiberized silk fiber, and then adding the fiberized silk fiber into the polyphenol-metal complex solution and stirring it, and then extracting alkali coordination after sufficient penetration to obtain the polyphenol-metal modified silk fiber; S3, washing the polyphenol-metal modified silk fiber obtained in step S2 with deionized water, and then adding bamboo pulp board and water for pulping to obtain slurry; S4, adding sizing agent and water to the slurry obtained in step S3, mixing and then sequentially performing sheet making, roller pressing and drying to obtain an antibacterial and aging-resistant paper-based material.
2. The method for preparing antibacterial and aging-resistant paper-based materials from polyphenol-modified silk fiber composite bamboo pulp according to claim 1, characterized in that: In step S1, the complex enzyme preparation includes the following components in parts by weight: 2-4 parts of papain, 1-3 parts of trypsin, 1-2 parts of pectinase, 2-4 parts of disodium hydrogen phosphate and 1-2 parts of sodium dihydrogen phosphate.
3. The method for preparing antibacterial and aging-resistant paper-based materials from polyphenol-modified silk fiber composite bamboo pulp according to claim 1, characterized in that: In step S1, the mass ratio of the complex enzyme preparation, raw silkworm cocoons and water is 1-2:250-350:9500-10500.
4. The method for preparing antibacterial and aging-resistant paper-based materials from polyphenol-modified silk fiber composite bamboo pulp according to claim 1, characterized in that: In step S1, the pH value is 8-10, the temperature is 45-55° C., and the stirring is 60-80 r / min. The stirring is performed for 4-6 minutes, and the stirring is stopped for 9-11 minutes. This is repeated 6-8 times.
5. The method for preparing antibacterial and aging-resistant paper-based material by using polyphenol-modified silk fiber composite bamboo pulp as claimed in claim 1, characterized in that: In step S2, the mass ratio of the fibrillated silk fibers to the polyphenol-metal complex solution is 1-2:18-22.
6. The method for preparing antibacterial and aging-resistant paper-based materials by using polyphenol-modified silk fiber composite bamboo pulp as claimed in claim 1 or 5, characterized in that: In step S2, the method for preparing the polyphenol-metal complex solution comprises the following steps: adding polyphenol and metal salt into a citric acid solution, and fully stirring the solution at room temperature to obtain a polyphenol-metal complex solution.
7. The method for preparing antibacterial and aging-resistant paper-based materials from polyphenol-modified silk fiber composite bamboo pulp according to claim 6, characterized in that: The polyphenol is at least one of epicatechin, epigallocatechin, epicatechin gallate and epigallocatechin gallate; the metal salt is at least one of aluminum salt, calcium salt, zinc salt, silver salt and titanium salt.
8. The method for preparing antibacterial and aging-resistant paper-based materials from polyphenol-modified silk fiber composite bamboo pulp according to claim 1, characterized in that: In step S2, the mixture is stirred at 35-50° C. and 60-80 r / min for 4-6 min and 9-11 min, and the stirring is repeated 6-8 times. Then, the pH value is adjusted to 5-7, and the mixture is stirred at 60-80 r / min for 4-6 min and 9-11 min, and the stirring is repeated 2-4 times before draining the mixture.
9. The method for preparing antibacterial and aging-resistant paper-based materials from polyphenol-modified silk fiber composite bamboo pulp according to claim 1, characterized in that: In step S4, the sizing agent is at least one of gelatin, starch, polyvinyl alcohol and carboxymethyl cellulose.
10. An antibacterial and aging-resistant paper-based material prepared by the method for preparing an antibacterial and aging-resistant paper-based material using polyphenol-modified silk fibroin fiber composite bamboo pulp as claimed in any one of claims 1 to 9.
Citation Information