Plasma treatment composite anti-corrosion coating metal hanging plate design for marine antifouling paint test and preparation method of plasma treatment composite anti-corrosion coating metal hanging plate design

Through plasma treatment and composite coating technology, the problem of poor corrosion resistance of metal hanging plates for antifouling coating tests in marine environments is solved, and high fastness and durability antifouling coating tests are achieved, and the coating and foundation are enhanced. The bonding effect and corrosion resistance of the material reduce the manufacturing difficulty and cost.

CN119000205APending Publication Date: 2024-11-22MINDONG HYDROPOWER DEV CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411090740.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing metal hanging boards for antifouling coatings are difficult to resist corrosion for a long time in marine environments, and the interface bonding performance between metal and organic coatings is poor, which affects the test results of antifouling coatings.

Method used

The surface of metal sample is cleaned and polished by plasma treatment technology, and coated with polyurethane-based graphene-modified anticorrosion coating and epoxy-based silicon-modified anticorrosion coating to form a composite anticorrosion coating to enhance the bonding with metal substrates. and improve corrosion resistance through double coating and nanomaterials.

Benefits of technology

It realizes long-term corrosion-resistant and high-fast anti-fouling coating test metal anti-corrosion hanging board, enhances the adhesion effect between the coating and the substrate, improves the durability and corrosion resistance to the marine environment, reduces the difficulty of manufacturing and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119000205A_ABST
    Figure CN119000205A_ABST
Patent Text Reader

Abstract

The invention relates to a plasma treatment composite anticorrosive coating metal hanging plate design for marine antifouling paint testing and a preparation method thereof. The metal hanging plate comprises stainless steel, aluminum alloy, low-carbon steel and the like, and the surface of the hanging plate is subjected to plasma treatment and composite anti-corrosion coating coating. The manufacturing method comprises the following specific steps: polishing and cleaning the sample plate; processing the sample plate by adopting plasma; sequentially spraying a polyurethane-based graphene modified anticorrosive coating and an epoxy-based silicon modified anticorrosive coating in airless spraying and other modes; the surface of the coating is treated by plasma to improve the interface bonding performance. And building a floating platform, and fixing the sample plate on the hanging plate by using an insulating rope to obtain the anti-corrosion hanging plate. The anti-corrosion hanging plate can be used for testing marine antifouling paint of a metal substrate. The anti-corrosion coating is simple in structure and easy to coat, and the anti-corrosion hanging plate prepared on the basis of the anti-corrosion coating is low in manufacturing difficulty, good in reliability and low in cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of marine hanging plates, and in particular to a design of a composite anti-corrosion coating metal hanging plate treated with plasma for testing marine anti-fouling coatings and a preparation method thereof. Background Art

[0002] Marine fouling refers to the damage to the anti-corrosion layer caused by various marine organisms such as animals, plants and microorganisms that attach to and inhabit the working ship equipment and marine engineering facilities in the marine environment, which accelerates the metal corrosion and shortens the service life of ships and marine structures. Biological fouling also increases fluid dynamic resistance, reduces ship maneuverability, and increases fuel consumption. Marine resources and marine industries have become an indispensable pillar of economic development, so the development of anti-fouling materials and protection technologies has become a global issue.

[0003] The most direct and effective test in the development of antifouling coatings is the real sea hanging board test. Due to the different environmental conditions in different sea areas, such as temperature, humidity, salinity, oxygen and pH value, as well as the significant differences in marine biological species, antifouling coatings must undergo real sea hanging board testing to verify their reliability before actual application. The hanging board used for testing antifouling coatings should first be treated with anti-corrosion. The adhesion strength, anti-corrosion effect and interface bonding of the hanging board anti-corrosion coating and the anti-fouling coating will have a significant impact on the performance test of the antifouling coating. Due to the poor interface bonding performance between metal and organic coating, it is difficult to provide long-term protection. Therefore, it is urgent to develop and design a metal anti-corrosion hanging board for antifouling coating testing with long-term corrosion resistance, high fastness and a roughened surface. Summary of the invention

[0004] The purpose of the present invention is to provide a metal anti-corrosion hanging plate for anti-fouling coating testing with long-term corrosion resistance, high fastness and roughened surface, and a preparation method thereof.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] Cleaning and polishing of metal sample surface: Before the metal sample is coated with anti-corrosion coating, its surface should be treated first to remove oil, soluble salt, floating dust, moisture and other contaminants on the coated surface, and then polished to roughen it. Finally, the dust on the sample should be cleaned to obtain a sample with a rough and clean surface.

[0007] Preferably, the surface dirt of the sample is first ultrasonically cleaned with acetone for 15-30 minutes, and then ultrasonically cleaned with deionized water for 3-5 times, each time for 5 minutes; the sample is treated with a high-pressure water gun, shot blasting or sand blasting to achieve the rust removal standard Sa2.5 level, and the roughness reaches 40-70um; the dust on the sample is cleaned by ultrasonic cleaning with ethanol and deionized water for 5 minutes respectively.

[0008] Plasma treatment of metal sample surface: After the metal sample surface is cleaned and polished, plasma treatment equipment is used to perform plasma treatment on the metal sample.

[0009] Preferably, the plasma treatment is carried out in an air atmosphere, the treatment power is selected to be 1000-3000 W, and the treatment time should be between 3-20 min.

[0010] Composite anti-corrosion coating on metal sample surface: polyurethane-based graphene-modified anti-corrosion coating and epoxy-silicon-modified anti-corrosion coating are sequentially applied on the surface of the surface-treated sample to construct a composite anti-corrosion coating.

[0011] Preferably, the surfaces of the polyurethane-based graphene-modified anti-corrosion coating and the epoxy-based silicon-modified anti-corrosion coating should be plasma treated; the plasma treatment is carried out in a nitrogen atmosphere, the treatment power is selected from 500-1500W, and the treatment time is selected from 3-10min.

[0012] Preferably, the mass fraction ratio of the polyurethane-based graphene-modified anti-corrosion coating formula is: 70-85% aqueous polyurethane emulsion; 7-15% polymethyl methacrylate; 5-10% epoxy resin; 0.5-3% graphene powder; and 0.1-1% dimethyl silicone oil.

[0013] Preferably, the formula of the epoxy-silicon modified anti-corrosion coating has the following mass fraction ratios: epoxy resin 50-75%; waterborne polyurethane emulsion 10-25%; polyvinyl chloride 3-5%; nano-silicon dioxide 2-7%; polydimethylsiloxane 5-8%; and dimethyl silicone oil 0.1-1%.

[0014] Preferably, the solid content of the aqueous polyurethane emulsion is 27-38%; the epoxy resin is selected from bisphenol A epoxy resin and amine curing agent; the single layer rate of the graphene powder is 70-99%, and the flake diameter is 100-500nm.

[0015] Optionally, the composite anti-corrosion coating is applied by one or more of airless spraying, brushing or roller coating.

[0016] Preferably, each layer of the composite anti-corrosion coating should be coated 2-3 times respectively, so that each layer reaches a dry film thickness of 300-400 μm.

[0017] Preferably, the polyurethane-based graphene-modified anti-corrosion coating should first be cured and dried at 90°C for 4 hours, and then cured at room temperature for 24-48 hours; the epoxy-based silicon-modified anti-corrosion coating should first be cured at room temperature for 24-48 hours, and then cured at 90°C for 2 hours.

[0018] Preferably, the relative humidity of the composite anti-corrosion coating construction environment should be controlled below 85%, and the substrate temperature should be at least 3°C ​​lower than its dew point temperature.

[0019] Preparation of anti-corrosion metal hanging plates for marine anti-fouling test: Build a floating platform in the test sea area. The size of the floating platform is determined according to the number and size of the test hanging plates. It is fixed by anchoring, and a metal or wooden frame is built on the floating platform to facilitate the fixing of the sample. Use insulating ropes to fix the four corners of the sample on the frame to obtain the anti-corrosion hanging plate.

[0020] Preferably, the floating platform is 5m-20m long and 3m-12m wide.

[0021] Preferably, the hanging plate frame has a length of 800mm-1600mm and a width of 400mm-1200mm.

[0022] Preferably, the length of the template is 100mm-400mm, the width is 50mm-200mm, and the thickness is 1mm-4mm; the diameter of the circular holes at the four corners for fixing the insulating rope is 2mm-6mm.

[0023] The beneficial effects of the present invention are:

[0024] 1. The present invention uses plasma to treat the surface of the metal substrate and the surface of the anti-corrosion coating, introduces oxygen-containing functional groups, and makes the anti-corrosion coating and the metal substrate, and the coatings have good adhesion. Plasma pretreatment of the outermost epoxy-silicon modified anti-corrosion coating surface can effectively improve the interface adhesion effect between the anti-fouling coating and the anti-corrosion coating in the hanging board test.

[0025] 2. Double-layer coating is adopted. Epoxy resin and polyurethane resin can provide excellent mechanical properties and resist physical erosion such as wave erosion; while the layered addition of nano-silica and graphene sheets can effectively block the corrosion of the marine environment, especially chloride ions, magnesium ions, etc. on metals.

[0026] 3. The thickness of the anti-corrosion coating can be controlled and determined by the number of coatings.

[0027] 3. The anti-corrosion coating of the present invention is simple to apply, has low environmental requirements, and is easy to operate.

[0028] 4. The anti-corrosion coating of the present invention has a simple structure and is easy to apply. The anti-corrosion hanging plate prepared based on the anti-corrosion coating has low manufacturing difficulty, good reliability and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a schematic diagram of the hanging board;

[0030] Figure 2 This is a sample schematic diagram;

[0031] In the accompanying drawings: 1-insulated wire, 2-sample, 3-frame, 4-counterweight, 5-substrate, 6-polyurethane-based graphene-modified anti-corrosion coating, 7-epoxy-silicon-modified anti-corrosion coating, 8-anti-fouling coating to be tested. Specific embodiments

[0032] Embodiment 1:

[0033] Stainless steel anti-corrosion specimens for marine anti-fouling testing

[0034] Cleaning and polishing of the surface of the stainless steel sample: The dirt on the surface of the sample is first ultrasonically cleaned with acetone for 15 minutes, and then ultrasonically cleaned with deionized water for 3 times, each time for 5 minutes; the sample is treated with a high-pressure water gun, shot blasting or sand blasting to achieve the rust removal standard Sa 2.5 level, and the roughness reaches 40-70um; the sample dust is cleaned by ultrasonic cleaning with ethanol and deionized water for 5 minutes respectively.

[0035] Surface plasma treatment of stainless steel samples: Surface plasma treatment of metal samples was carried out in an air atmosphere, the processing power was 2000W, and the processing time was 5min.

[0036] Composite anti-corrosion coating on the surface of stainless steel sample: spray polyurethane-based graphene-modified anti-corrosion coating and epoxy-silicon-modified anti-corrosion coating on the surface of the surface-treated sample in sequence to construct a composite anti-corrosion coating. The surfaces of the polyurethane-based graphene-modified anti-corrosion coating and epoxy-silicon-modified anti-corrosion coating should be plasma-treated; the plasma treatment is carried out in a nitrogen atmosphere, the treatment power is 1000W, and the treatment time is 3min. The mass fraction ratio of the polyurethane-based graphene-modified anti-corrosion coating formula is: 80% water-based polyurethane emulsion; 11% polymethyl methacrylate; 6% epoxy resin; 2.5% graphene powder; 0.5% dimethyl silicone oil. The mass fraction ratio of the epoxy-silicon-modified anti-corrosion coating formula is: 70% epoxy resin; 15% water-based polyurethane emulsion; 3% polyvinyl chloride; 5% nano-silicon dioxide; 6.5% polydimethylsiloxane; 0.5% dimethyl silicone oil. The solid content of the aqueous polyurethane emulsion is 38%; the epoxy resin is selected from bisphenol A epoxy resin and amine curing agent; the single layer rate of the graphene powder is 80%, and the sheet diameter is 300nm.

[0037] The composite anti-corrosion coating is applied by airless spraying. Each layer of the composite anti-corrosion coating should be applied twice respectively, so that each layer reaches a dry film thickness of 300-400 μm.

[0038] The polyurethane-based graphene-modified anti-corrosion coating should be cured and dried at 90°C for 4 hours, and then cured at room temperature for 24 hours; the epoxy-based silicon-modified anti-corrosion coating should be cured at room temperature for 48 hours, and then cured at 90°C for 2 hours. The relative humidity of the composite anti-corrosion coating construction environment should be controlled below 85%, and the substrate temperature should be 3°C lower than its dew point temperature.

[0039] Preparation of metal / concrete mixed substrate anti-corrosion hanging board for marine antifouling test: A floating platform is built in the test sea area. The size of the floating platform is 10m long and 6m wide. It is fixed by anchoring, and a metal frame is built on the floating platform to facilitate the fixing of the sample. The four corners of the sample are fixed to the frame with insulating ropes to simulate underwater floating conditions. The hanging board frame is 1200mm long and 800mm wide. The length of a single sample is 200mm, the width is 100mm, and the thickness is 2mm; the diameter of the circular holes at the four corners for fixing the insulating ropes is 4mm.

[0040] Embodiment 2:

[0041] Aluminum alloy anti-corrosion sample for marine antifouling test

[0042] Surface cleaning and polishing of aluminum alloy samples: The surface dirt of the sample is first ultrasonically cleaned with acetone for 20 minutes, and then ultrasonically cleaned with deionized water for 3 times, each time for 5 minutes; the sample is treated with high-pressure water gun, shot blasting or sand blasting to reach the rust removal standard Sa 2.5 level, and the roughness reaches 40-70um; the sample dust is cleaned by ultrasonic cleaning with ethanol and deionized water for 5 minutes respectively.

[0043] Surface plasma treatment of aluminum alloy samples: The surface plasma treatment of metal samples was carried out in an air atmosphere, the processing power was 1500W, and the processing time was 8min.

[0044] Composite anti-corrosion coating on the surface of aluminum alloy sample: spray polyurethane-based graphene-modified anti-corrosion coating and epoxy-silicon-modified anti-corrosion coating on the surface of the surface-treated sample in sequence to construct a composite anti-corrosion coating. The surfaces of the polyurethane-based graphene-modified anti-corrosion coating and epoxy-silicon-modified anti-corrosion coating should be plasma-treated; the plasma treatment is carried out in a nitrogen atmosphere, the treatment power is 1500W, and the treatment time is 3min. The mass fraction ratio of the polyurethane-based graphene-modified anti-corrosion coating formula is: 75% water-based polyurethane emulsion; 13% polymethyl methacrylate; 9% epoxy resin; 2.5% graphene powder; 0.5% dimethyl silicone oil. The mass fraction ratio of the epoxy-silicon-modified anti-corrosion coating formula is: 65% epoxy resin; 18% water-based polyurethane emulsion; 5% polyvinyl chloride; 5% nano-silicon dioxide; 6.5% polydimethylsiloxane; 0.5% dimethyl silicone oil. The solid content of the aqueous polyurethane emulsion is 38%; the epoxy resin is selected from bisphenol A epoxy resin and amine curing agent; the single layer rate of the graphene powder is 85%, and the sheet diameter is 500nm.

[0045] Preparation of metal / concrete mixed substrate anti-corrosion hanging board for marine antifouling test: A floating platform is built in the test sea area. The size of the floating platform is 20m long and 12m wide. It is fixed by anchoring, and a metal frame is built on the floating platform to facilitate the fixing of the sample. The four corners of the sample are fixed to the frame with insulating ropes to simulate underwater floating conditions. The hanging board frame is 1600mm long and 1200mm wide. The length of a single sample is 400mm, the width is 200mm, and the thickness is 4mm; the diameter of the circular holes at the four corners for fixing the insulating ropes is 6mm.

[0046] The anticorrosive coatings and samples thereof in Examples 1 and 2 were selected, and salt spray resistance test, aging resistance test, salt water resistance test and pull-off adhesion test were performed respectively according to standards GB / T1771-2007, GB / T 1865-2009, GB / T 10834-2008 and GB / T5210-2006. The test results are as follows:

[0047] Table 1 Test results of anti-corrosion coatings' resistance to salt spray, salt water and aging performance

[0048]

[0049] Both anti-corrosion coatings have good resistance to salt spray and salt water. After 2000h of testing, both coatings have intact paint films without blistering, shedding and corrosion. After 1500h of aging resistance test, both anti-corrosion coatings showed no powdering or cracking, and the paint films were intact, indicating good aging resistance; the coating of Example 1 changed color by level 1, and the coating of Example 2 did not change color, both showing good color fastness. The pull-out adhesion strength between the anti-corrosion coating and the stainless steel substrate in Example 1 reached 10.58MPa, and the pull-out adhesion strength between the anti-corrosion coating and the aluminum alloy substrate in Example 2 reached 6.89MPa, showing excellent bonding strength.

[0050] The anti-corrosion effects of the anti-corrosion panels of Examples 1 and 2 in actual sea tests are as follows:

[0051] Table 2 Anticorrosion effect of hanging board

[0052]

[0053] The hanging plates of Examples 1 and 2 showed good anti-corrosion effects in the actual sea test, without paint peeling or rust. The surface of the anti-corrosion samples was not treated with anti-fouling, so it is normal for marine organisms to attach to the surface.

Claims

1. A plasma-treated composite anti-corrosion coating metal hanging plate for testing marine anti-fouling coatings, characterized in that: The metal cladding substrate includes but is not limited to low carbon steel, stainless steel and aluminum alloy.

2. The plasma-treated composite anti-corrosion coating metal hanging plate for testing marine anti-fouling coatings according to claim 1, characterized in that: The surface of the cladding substrate needs to be polished, cleaned and plasma treated.

3. The plasma treatment according to claim 2, characterized in that: The atmosphere should be air, the processing power should be 1000-3000W, and the processing time should be between 3-20min.

4. The plasma-treated composite anti-corrosion coating metal hanging plate for testing marine anti-fouling coatings according to claim 1, characterized in that: The hanging plate adopts a composite anti-corrosion coating structure, which comprises a polyurethane-based graphene-modified anti-corrosion coating and an epoxy-based silicon-modified anti-corrosion coating from the inside to the outside.

5. The composite anti-corrosion coating according to claim 4, characterized in that: After each layer of anti-corrosion coating is applied, plasma treatment should be used.

6. The plasma treatment according to claim 5, characterized in that: The atmosphere is nitrogen, the processing power is 500-1500W, and the processing time is 3-10min.

7. The polyurethane-based graphene-modified anti-corrosion coating according to claim 4, characterized in that: The mass fraction ratio of the components is: 70-85% of waterborne polyurethane emulsion; 7-15% of polymethyl methacrylate; 5-10% of epoxy resin; 0.5-3% of graphene powder; 0.1-1% of dimethyl silicone oil; the curing conditions are: curing and drying at 90°C for 4 hours, and then curing at room temperature for 24-48 hours.

8. The epoxy-silicon modified anti-corrosion coating according to claim 4, characterized in that: The mass fraction ratio of the components is: epoxy resin 50-75%; water-based polyurethane emulsion 10-25%; polyvinyl chloride 3-5%; nano silicon dioxide 2-7%; polydimethylsiloxane 5-8%; dimethyl silicone oil 0.1-1%; The curing conditions are: curing at room temperature for 24-48 hours, and then curing at 90°C for 2 hours.

9. The anticorrosive coating formulation according to claim 7-8, characterized in that: The solid content of the aqueous polyurethane emulsion is 27-38%; the epoxy resin is selected from bisphenol A epoxy resin and amine curing agent; the single layer rate of the graphene powder is 70-99%, and the sheet diameter is 100-500nm.

10. The composite anti-corrosion coating design according to claim 4 is characterized by: Each coating should be sprayed 2-3 times to achieve a dry film thickness of 300-400μm.