NiO and WO3 heterojunction xylene gas sensor prepared based on electrostatic spinning method, preparation process and application
A NiO/WO3 heterojunction nanofiber gas sensor was prepared by electrospinning, which solved the limitations of existing sensors in xylene detection in terms of sensitivity and response time, and achieved high sensitivity and fast response xylene detection effect.
Patent Information
- Application Number
- CN202411389457.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-11-22
AI Technical Summary
Existing single-material gas sensors have limitations in terms of sensitivity, selectivity, and response time when detecting xylene, making it difficult to meet the requirements for high sensitivity, high selectivity, and fast response.
NiO/WO3 heterojunction nanofiber gas sensors were prepared by electrospinning. Suitable oxide heterojunctions were constructed, and the phase composition and microstructure were optimized to form a uniformly distributed pn heterojunction structure.
It achieves highly sensitive detection of xylene, with an extremely low detection limit and fast response recovery time, making it suitable for environmental monitoring and industrial safety.
Smart Images

Figure CN119000802A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electronic components, and in particular relates to a xylene gas sensor having a NiO and WO3 heterojunction prepared by an electrospinning method, a preparation process and an application thereof. Background Art
[0002] With the continuous advancement of industrialization, emissions of volatile organic compounds (VOCs) have increased annually, posing a serious threat to the environment and human health. Xylene, a common VOC, is widely used in solvents, coatings, paints, and petrochemical products. Long-term exposure to high concentrations of xylene can adversely affect the human nervous system, respiratory system, and organs such as the liver. Therefore, the development of a highly sensitive, selective, and fast-response xylene detection method is of great practical significance.
[0003] Currently, gas sensors are one of the primary means of detecting VOCs. Semiconductor metal oxide (SMO) gas sensors have attracted widespread attention and application due to their excellent gas sensitivity, stability, and cost-effectiveness. Nickel oxide (NiO), a p-type semiconductor material, has been widely used in gas sensing due to its excellent properties in gas adsorption and reaction. Tungsten trioxide (WO3), a typical n-type semiconductor material, also plays an important role in gas sensing applications due to its excellent electrical properties and chemical stability. However, single-material gas sensors still have certain limitations in terms of sensitivity, selectivity, and response time.
[0004] In recent years, composite sensors based on pn heterojunctions have become a research hotspot. By combining p-type and n-type semiconductor materials, a pn heterojunction can be formed. This structure can significantly improve the sensitivity and selectivity of the sensor, while also improving its response time and stability. For example, (Chenhao Wang, Shendan Zhang, Lei Qiu, et al. Ru-decorated WO3 nanosheets for efficient xylene gas sensing application, Alloys and Compounds 22 (2020) 154196) et al. modified WO3 nanosheets with Ru, significantly enhancing their response to xylene. They demonstrated high sensitivity and excellent selectivity for xylene in the modified WO3. (Li Liua, Yu Zhang, Guoguang Wang, et al. High toluene sensing properties of NiO–SnO2 composite nanofiber sensors operating at 330°C, Sens. Actuators B Chem. (2011)) et al. modified SnO2 nanowires with NiO, significantly improving the performance of SnO2 and exhibiting good selectivity and response to xylene. This shows that the formation of heterojunction can improve the sensing performance of semiconductor materials. It also shows that the addition of NiO improves the response value, response / recovery speed and stability, and is an excellent additive.
[0005] Electrospinning, as a method for producing nanofibers, offers advantages such as simplicity, low cost, and high controllability. Electrospinning can produce large, uniform, and porous nanofiber structures, providing more active sites for the adsorption and diffusion of gas molecules, significantly improving the performance of gas sensors. In particular, controlling spinning parameters and post-processing techniques can achieve uniform distribution and close bonding of different materials, forming an excellent pn heterojunction structure.
[0006] Based on the above situation, we proposed a nanofiber gas sensor based on a NiO / WO3 heterojunction, fabricated via electrospinning, and systematically investigated its structure and performance. Experimental results demonstrated that the sensor exhibited excellent sensitivity and an ultra-low detection limit for xylene, demonstrating its potential value in practical applications.
[0007] Therefore, this patent aims to provide a high-performance xylene gas sensor based on NiO / WO3 heterojunction nanofibers, in order to play an important role in environmental monitoring, industrial safety and public health. Summary of the Invention
[0008] The purpose of the present invention is to provide a xylene gas sensor and a detection method thereof with good response, low detection limit and good selectivity by constructing a suitable oxide heterojunction, optimizing the phase composition, and designing a microstructure with adjustable size and morphology.
[0009] The technical solution of the present invention:
[0010] A xylene gas sensor with a NiO and WO3 heterojunction prepared by electrospinning. The ammonia gas sensor mainly consists of a gas-sensitive material and a ceramic tube. The gas-sensitive material is coated on the surface of the ceramic tube with a coating thickness of 40μm to 80μm. The gas-sensitive material is composed of a nickel oxide and tungsten oxide heterojunction composite nanomaterial.
[0011] The nickel oxide and tungsten oxide heterojunction composite nanomaterial is prepared into nanofibers through an electrostatic spinning method.
[0012] The surface of the ceramic tube is provided with a platinum wire lead with a size of 4*1.35*0.35 mm and a high temperature resistance of below 800°C.
[0013] A preparation process for a xylene gas sensor based on a NiO and WO3 heterojunction prepared by electrospinning, comprising the following steps:
[0014] (1) Dissolve ammonium metatungstate in DMF solution and stir magnetically for 10 min to fully dissolve it to form a uniform solution. Weigh nickel chloride hexahydrate and add it to the solution, controlling the molar ratio of Ni to W to be 0.2% to 0.4%. Stir at 40°C for 1 to 2 h, then add PVP and continue stirring for 3 h until a uniform and transparent precursor spinning solution is formed.
[0015] (2) A transparent spinning solution is drawn into the syringe, free of air bubbles, and fixed to a propeller. The needle is connected to the positive electrode of a DC power supply. The propeller speed is set to 80 μL / min to push the liquid out. The humidity of the electrospinning environment is maintained at 20%, the distance between the needle and the collection plate is 20 cm, and the DC power supply provides a static voltage of 22 kV. Finally, the spinning solution is drawn into nanofilaments under the action of the electric field and collected on a collection plate.
[0016] (3) The nanowires were collected into a porcelain boat and placed in a tube furnace for calcination. The starting temperature was 30°C, the heating rate was 2°C / min, and the temperature was kept at 500°C for 2h. The temperature was then naturally cooled to obtain a xylene gas sensor.
[0017] NiO and WO3 heterojunction gas sensors prepared by electrospinning are used to detect xylene gas, and their working environment temperature is 200℃ to 400℃.
[0018] Working principle of the present invention:
[0019] The xylene gas sensor of this invention is a resistive semiconductor gas sensor. It primarily utilizes the redox reaction that occurs on the semiconductor surface when it comes into contact with the gas being measured, causing changes in carrier concentration and, in turn, in the semiconductor's resistance. This change reflects the type and concentration of the gas being measured. The xylene gas sensor is made of NiO / WO3. When xylene gas molecules adsorb onto the surface, they cause changes in the electronic state of the NiO / WO3 surface, leading to changes in the semiconductor's conductivity. The sensor's real-time monitoring signal is the change in sensor resistance.
[0020] Beneficial effects of the present invention:
[0021] (1) The present invention adopts an electrospinning method to obtain a novel heterojunction composite nanomaterial. The raw materials are easy to obtain and inexpensive, and the heterojunction preparation process is simple. It is a metal oxide semiconductor heterojunction preparation solution with small equipment investment and simple process flow.
[0022] (2) The NiO / WO3 heterojunction composite-based sensor prepared in this invention exhibits high sensitivity in detecting xylene gas, producing a significant resistance change in response to extremely low concentrations of xylene. This means that the sensor can quickly and accurately detect extremely low levels of xylene in the environment, helping to promptly identify potential xylene contamination.
[0023] (3) The present invention significantly reduces the sensor's response recovery time. Because NiO / WO3 has excellent adsorption and desorption capabilities for xylene, the sensor typically has a fast response time. Once the xylene concentration in the environment changes, the NiO / WO3 sensor quickly responds and outputs a corresponding signal, enabling the monitoring system to react promptly. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a scanning electron microscope microscopic morphology of the NiO / WO3 nanocomposite material of the present invention.
[0025] Figure 2 This is the response value curve of the NiO / WO3 nanocomposite gas sensor with different ratios to 1 ppm xylene.
[0026] Figure 3 This is the response curve of NiO / WO3 nanocomposite gas sensor under different xylene concentrations.
[0027] Figure 4 The response values of NiO / WO3 nanocomposite gas sensors to seven gases at 1 ppm. DETAILED DESCRIPTION
[0028] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and technical solutions.
[0029] Example 1
[0030] (1) 0.5 mmol of ammonium metatungstate was dissolved in 5 mL of DMF solution and magnetically stirred for 10 min to fully dissolve it to form a uniform solution. 0.0033 mmol of nickel chloride hexahydrate was weighed and added thereto. The solution was stirred at 40 °C for 1 h. Then, 10 wt% of PVP was added and the solution was stirred for 3 h until a uniform and transparent spinning solution was formed.
[0031] (2) Aspirate the transparent spinning solution into a 5 mL syringe, remove any bubbles, and secure it to a propeller. Connect the needle to the positive electrode of a DC power supply. Set the propeller speed to 80 μL / min to push the liquid out. Maintain the humidity of the electrospinning environment at approximately 20%. The distance between the needle and the collection plate is 20 cm, and the DC power supply provides a static voltage of 22 kV. Finally, the solution is drawn into nanofilaments under the action of the electric field and collected on a collection plate.
[0032] (3) The nanowires were collected into a porcelain boat and placed in a tube furnace for calcination. The starting temperature was 30 °C, the heating rate was 2 °C / min, and the temperature was kept at 500 °C for 2 h, followed by natural cooling.
[0033] (4) Grinding the NiO / WO3 nanocomposite material into powder, dispersing the ground NiO / WO3 nanocomposite material powder into deionized water, and evenly coating the powder on the surface of the ceramic tube with a brush. The powder is placed in a drying oven at 60°C for about 10 hours, and then naturally cooled to room temperature to obtain a NiO / WO3 nanocomposite material gas sensor.
[0034] Example 2
[0035] (1) 0.5 mmol of ammonium metatungstate was dissolved in 5 mL of DMF solution and magnetically stirred for 10 min to fully dissolve it to form a uniform solution. 0.005 mmol of nickel chloride hexahydrate was weighed and added thereto. The solution was stirred at 40 °C for 1 h. Then, 10 wt% of PVP was added and the solution was stirred for 3 h until a uniform and transparent spinning solution was formed.
[0036] (2) Aspirate the transparent spinning solution into a 5 mL syringe, remove any bubbles, and secure it to a propeller. Connect the needle to the positive electrode of a DC power supply. Set the propeller speed to 80 μL / min to push the liquid out. Maintain the humidity of the electrospinning environment at approximately 20%. The distance between the needle and the collection plate is 20 cm, and the DC power supply provides a static voltage of 22 kV. Finally, the solution is drawn into nanofilaments under the action of the electric field and collected on a collection plate.
[0037] (3) The nanowires were collected in a porcelain boat and calcined in a tube furnace. The starting temperature was 30°C, the temperature was increased at a rate of 2°C / min, and the temperature was maintained at 500°C for 2 h, followed by natural cooling. To ensure sufficient calcination, the material was transferred from the collection plate to the porcelain boat using tweezers and spread flat on the bottom of the boat.
[0038] (4) Grinding the NiO / WO3 nanocomposite material into powder, dispersing the ground NiO / WO3 nanocomposite material powder into deionized water, and evenly coating the powder on the surface of the ceramic tube with a brush. The powder is placed in a drying oven at 60°C for about 10 hours, and then naturally cooled to room temperature to obtain a NiO / WO3 nanocomposite material gas sensor.
[0039] Example 3
[0040] (1) 0.5 mmol of ammonium metatungstate was dissolved in 5 mL of DMF solution and magnetically stirred for 10 min to fully dissolve it to form a uniform solution. 0.0066 mmol of nickel chloride hexahydrate was weighed and added thereto. The solution was stirred at 40 °C for 1 h. Then, 10 wt% of PVP was added and the solution was stirred for 3 h until a uniform and transparent spinning solution was formed.
[0041] (2) Aspirate the transparent spinning solution into a 5 mL syringe, remove any bubbles, and secure it to a propeller. Connect the needle to the positive electrode of a DC power supply. Set the propeller speed to 80 μL / min to push the liquid out. Maintain the humidity of the electrospinning environment at approximately 20%. The distance between the needle and the collection plate is 20 cm, and the DC power supply provides a static voltage of 22 kV. Finally, the solution is drawn into nanofilaments under the action of the electric field and collected on a collection plate.
[0042] (3) The nanowires were collected into a porcelain boat and placed in a tube furnace for calcination. The starting temperature was 30 °C, the heating rate was 2 °C / min, and the temperature was kept at 500 °C for 2 h, followed by natural cooling.
[0043] (4) Grinding the NiO / WO3 nanocomposite material into powder, dispersing the ground NiO / WO3 nanocomposite material powder into deionized water, and evenly coating the powder on the surface of the ceramic tube with a brush. The powder is placed in a drying oven at 60°C for about 10 hours, and then naturally cooled to room temperature to obtain a NiO / WO3 nanocomposite material gas sensor.
Claims
1. A xylene gas sensor based on the preparation of NiO and WO3 heterojunction by electrospinning, characterized in that: The xylene gas sensor is mainly composed of a gas-sensitive material and a ceramic tube. The gas-sensitive material is coated on the surface of the ceramic tube with a coating thickness of 40 μm to 80 μm. The gas-sensitive material is composed of a heterojunction composite nanomaterial of nickel oxide and tungsten oxide.
2. The xylene gas sensor according to claim 1, characterized in that: The nickel oxide and tungsten oxide heterojunction composite nanomaterial is made into nanofibers by electrostatic spinning.
3. The xylene gas sensor according to claim 1, characterized in that: The surface of the ceramic tube is provided with a platinum wire lead, the size of which is 4*1.35*0.35 mm, and the high temperature resistance is below 800°C.
4. A preparation process for a xylene gas sensor based on a NiO and WO3 heterojunction prepared by electrospinning, characterized in that: The following steps are involved: (1) dissolving ammonium metatungstate in DMF solution, stirring magnetically for 10 min to fully dissolve it to form a uniform solution, then adding nickel chloride hexahydrate, controlling the molar ratio of Ni to W to be 0.2% to 0.4%, stirring at 40° C. for 1 to 2 h, then adding PVP, and continuing to stir for 3 h until a uniform and transparent precursor spinning solution is formed; (2) The precursor spinning solution is sucked into the syringe, the bubbles therein are exhausted, and the syringe is fixed on the propeller, and the positive electrode of the DC power supply is connected to the needle; the propeller speed is set to 80uL / min to push out the liquid, the humidity of the electrospinning environment is maintained at 20%, the distance between the needle and the collecting plate is 20cm, and the DC power supply provides a static voltage of 22kV; The precursor spinning solution is drawn into nanofilaments under the action of the electric field and collected on a collecting plate; (3) The nanowires were collected into a porcelain boat and placed in a tube furnace for calcination. The starting temperature of the calcination was 30°C, the heating rate was 2°C / min, and the temperature was kept at 500°C for 2h. The temperature was then naturally cooled to obtain a xylene gas sensor.
5. The xylene gas sensor according to claim 1 is used to detect xylene gas, and its working environment temperature is 200°C to 400°C.
Citation Information
Patent Citations
Cr2O3 or NiO porous film material using WO3 as base material and method for manufacturing air-sensitive sensor
CN102248737A
W6+doped NiO oxide semiconductor xylene sensor, manufacturing method and application thereof
CN104880492A
Porous semiconductor metal oxide complex nanofibers including nanoparticle catalyst functionalized by nano-catalyst included within metal-organic framework, gas sensor and member using the same, and method of manufacturing the same
US20170003272A1
Cited By
Preparation method of NiO-based 2-chloroethyl ethyl sulfide gas sensor
CN119915870A
Sulfur dioxide gas sensor and preparation method thereof
CN122545609A