Method for testing performance of metal amino hydrogen storage material

Through the combination of thermogravimetric analysis and gas chromatography-mass spectrometer, the ammonia release amount of metal amino hydrogen storage materials is quickly evaluated, solving the problem of excessive reversibility in the prior art, and achieving rapid , efficient material screening and data acquisition.

CN119001050AActive Publication Date: 2024-11-22CRINM (GUANGDONG) INST FOR ADVANCED MATERIALS & TECH

Patent Information

Application Number
CN202411478112.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-22
Publication Date
2024-11-22
Estimated Expiration
2044-10-22

AI Technical Summary

Technical Problem

In the prior art, it takes too long to evaluate the reversibility of metal amino hydrogen storage materials, and hundreds or thousands of cycles are required to obtain a sufficient sample size, resulting in inefficient evaluation.

Method used

Using a combination of thermogravimetric analysis and gas chromatography-mass spectrometer, the associated gas is collected through the thermogravimetric analyzer and transported to the gas chromatography-mass spectrometer for analysis, and the ammonia release amount is calculated to quickly evaluate the absorption and discharge of materials. Hydrogen reversibility.

Benefits of technology

This method can analyze the ammonia release amount of metal amino acid samples within 1 hour to 3 hours, reduce the test time, and only 20mg to 100mg samples can obtain rich data information, preliminary judgment of the reversibility of the material and assist in research Its thermal decomposition process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119001050A_ABST
    Figure CN119001050A_ABST
Patent Text Reader

Abstract

The invention discloses a method for testing the performance of a metal amino hydrogen storage material, which belongs to the field of chemical analysis, and comprises the following steps: taking a sample for thermogravimetric analysis, and collecting associated gas from a thermogravimetric analyzer at a weightlessness temperature point; respectively conveying the associated gases collected at the plurality of weightlessness temperature points into a gas chromatograph-mass spectrometer, and analyzing according to a preset gas chromatograph-mass spectrometer analysis program to generate a plurality of sample thermal decomposition gas maps; the method comprises the following steps: selecting a sample thermal decomposition gas spectrum generated by ammonia gas, extracting an ion chromatogram with a mass-to-charge ratio of 17 from the sample thermal decomposition gas spectrum, calculating a first peak area of an ammonia gas mass spectrum signal, and calculating the ammonia gas release amount. According to the method, the ammonia release amount of the metal amino substance sample at different temperatures can be analyzed only by 1-3 hours, the hydrogen absorption and desorption reversibility of the metal amino substance hydrogen storage material can be judged from another angle, and rich data information can be obtained only by 20-100 mg of sample in one test.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for testing the performance of a metal amide hydrogen storage material, and belongs to the field of chemical analysis. Background Art

[0002] With the development of industry and the improvement of people's material living standards, the demand for energy is also increasing day by day. Hydrogen energy, as a green energy with abundant reserves, wide sources and high energy density, is attracting widespread attention. The entire hydrogen economic process includes many aspects such as hydrogen production, storage and transportation, fuel cell application, safety, and performance index formulation. Hydrogen is produced through green energy such as wind energy and solar energy, and then hydrogen is used as fuel in fuel cells or hydrogen internal combustion engines to release energy. The whole process is clean, low-carbon, and does not produce additional pollutants. In terms of hydrogen production and hydrogen utilization, there are relatively mature technologies, and hydrogen storage is the bottleneck restricting the entire hydrogen energy cycle.

[0003] Hydrogen exists in three forms: gaseous, liquid and solid hydride. Based on this characteristic, people have developed three types of oxygen storage technologies, namely high-pressure gaseous hydrogen storage, low-temperature liquid hydrogen storage and solid hydrogen storage of hydrogen-containing materials. Solid-state hydrogen storage is considered to be the most promising hydrogen storage method due to its advantages such as high density and low cost. At present, among many solid-state hydrogen storage materials, metal amide composite system hydrogen storage materials have attracted much attention due to their high hydrogen storage capacity and more suitable thermodynamic properties of hydrogen absorption and desorption.

[0004] The main parameters for measuring the performance of solid-state hydrogen storage materials are hydrogen storage volume density, mass fraction, reversibility of hydrogen addition and desorption, hydrogen addition and desorption rate, and cyclic service life. In the prior art, if the reversibility of hydrogen addition and desorption of hydrogen storage materials is to be evaluated, the PCT curve and hydrogen absorption and desorption kinetic curve cycle test can be carried out by referring to GB / T 33291-2016 "Pressure-Composition-Isotherm (PCT) Test Method for Reversible Hydrogen Absorption and Desorption of Hydride", and the reversibility of hydrogen addition and desorption of hydrogen storage materials can be reflected by comparing the changes in hydrogen absorption and desorption capacity under different cycles. A cycle test of metal nitrogen hydride hydrogen storage materials takes about 4 hours. In order to obtain a sufficient sample volume, it must be cycled hundreds or thousands of times. This evaluation method is too time-consuming. Summary of the invention

[0005] In order to overcome the deficiencies of the prior art, the present invention provides a method for testing the performance of metal amide hydrogen storage materials, which can test the reversibility of metal amide hydrogen storage materials more quickly from another perspective.

[0006] The technical solution adopted by the present invention to solve its technical problem is: A method for testing the performance of a metal amide hydrogen storage material comprises the following steps: Take a sample and perform thermogravimetric analysis according to a preset thermogravimetric analysis program, and collect associated gas from the thermogravimetric analyzer at the weight loss temperature point; The associated gases collected at the plurality of weight loss temperature points are respectively transported to a gas chromatography-mass spectrometer, and analyzed according to a preset gas chromatography-mass spectrometry analysis program, and a sample thermal decomposition gas spectrum is generated for the associated gases corresponding to each weight loss temperature point; The thermal decomposition gas spectrum of the sample with ammonia produced is selected, and the ion chromatogram with a mass-to-charge ratio of 17 is extracted therefrom. The first peak area of ​​the ammonia mass spectrum signal at the corresponding weightlessness temperature point is calculated, and the ammonia release amount is calculated.

[0007] The metal amide hydrogen storage material performance testing method provided in the present application can analyze the ammonia release of metal amide samples at different temperatures in only 1 to 3 hours, which is conducive to screening out materials with better reversibility of hydrogen absorption and desorption according to the ammonia release amount; moreover, only 20 mg to 100 mg of sample is needed for one test to obtain rich data information, which is convenient for further research on the material.

[0008] Furthermore, the step of collecting associated gas from the thermogravimetric analyzer includes: The associated gas in the thermogravimetric analyzer is transported to a gas sample storage device via a first pipeline, and the associated gas collected at different weight loss temperature points is stored in different partitions; The step of respectively transporting the associated gases collected at the plurality of weightlessness temperature points to a gas chromatography-mass spectrometer comprises: The associated gas in the plurality of partitions is transported in batches to a gas chromatograph-mass spectrometer via a second pipeline.

[0009] When collecting associated gases at different weightlessness temperature points, only the associated gases at the moment of passing the weightlessness temperature point are collected, then stored in partitions, and finally subjected to gas chromatography-mass spectrometry analysis. This helps to ensure the continuity of the experiment and can accurately distinguish the components produced by the thermal decomposition of the sample at each weightlessness temperature point.

[0010] Furthermore, the first pipeline, the second pipeline and the gas sample storage are all kept at 200° C., which is conducive to the thermal decomposition products to maintain the component ratio just after the thermal decomposition as much as possible.

[0011] Furthermore, the step of taking samples and performing thermogravimetric analysis according to a preset thermogravimetric analysis program, and collecting associated gas from the thermogravimetric analyzer at the weight loss temperature point includes: Take two portions of metal amide type hydrogen storage material; The first material is subjected to thermogravimetric analysis according to the preset thermogravimetric analysis program to obtain a TG curve and a DSC curve, and the temperature at which the TG curve begins to lose weight is taken as the starting point, and the temperature at which the exothermic process of the DSC curve ends is taken as the end point, to obtain the temperature range of weight loss before decomposition of the sample; Selecting a plurality of weight loss temperature points within the weight loss temperature range before decomposition; The second material is used as the sample, and a thermogravimetric analysis is performed according to the preset thermogravimetric analysis program, and associated gas is collected from the thermogravimetric analyzer at multiple weight loss temperature points.

[0012] That is, in a complete experiment, the first material is only subjected to thermogravimetric analysis, and the second material is first subjected to thermogravimetric analysis and then to gas chromatography-mass spectrometry. The role of the first material is to indicate in advance at what temperature the metal amide to be tested begins to decompose and within what temperature range the thermogravimetric loss occurs, so as to facilitate the determination of the weight loss temperature point; the first material does not need to collect gas analysis, so the mass of the first material can be less than that of the second material.

[0013] Furthermore, in the step of selecting a plurality of weight loss temperature points within the weight loss temperature range before decomposition, the selection requirements satisfy: The extreme low value and the extreme high value of the weight loss temperature point span more than 60% of the preset temperature range and span the continuous endothermic-exothermic peak of the DSC curve; The preset temperature range starts at the temperature at which the sample starts to lose weight and ends at the end temperature of the continuous endothermic-exothermic peak in the DSC curve.

[0014] Furthermore, the step of calculating the ammonia release amount includes: Substituting the first peak area into a calibration equation to obtain the ammonia release amount; The step of obtaining the correction equation comprises: Taking standard substances of different masses into groups and performing thermogravimetric analysis according to the preset thermogravimetric analysis program, collecting multiple groups of product gases from the thermogravimetric analyzer; The product gases of each group are respectively transported to a gas chromatography-mass spectrometer, and analyzed according to a preset gas chromatography-mass spectrometry analysis program to obtain a thermal decomposition gas spectrum of a standard substance, and compared with a standard spectrum library to obtain a chromatographic peak position of ammonia in the thermal decomposition gas spectrum of the standard substance, and an ion chromatogram with a mass-to-charge ratio of 17 is extracted to obtain a second peak area of ​​ammonia mass spectrum signal; The theoretical ammonia mass generated by the thermal decomposition of the standard substance is used as the independent variable, the second peak area is used as the dependent variable, and the least square method is used to perform linear regression equation fitting to obtain the correction equation.

[0015] The standard spectrum library can be the NIST spectrum library.

[0016] Furthermore, the step of selecting the thermal decomposition gas spectrum of the sample in which ammonia is produced comprises: According to the retention time of the chromatographic peak position of ammonia in the thermal decomposition gas spectrum of the standard substance, the thermal decomposition gas spectrum of the sample in which ammonia is produced is selected.

[0017] Furthermore, the method for testing the performance of the metal amide hydrogen storage material further comprises: Comparing the thermal decomposition gas spectrum of the sample with the standard spectrum library to determine the gas composition of the sample decomposed at the weightlessness temperature point is conducive to simply analyzing the reversibility of hydrogen absorption and desorption of the material in one experiment, and incidentally analyzing more parameters in the thermal decomposition process of the material.

[0018] Furthermore, the standard substance is ammonium bicarbonate. Ammonium bicarbonate has a low thermal decomposition temperature and a fast thermal decomposition rate, and the decomposed gas is a mixed gas with simple components, which is conducive to determining the retention time of ammonia generated by thermal decomposition when doing gas chromatography, and is conducive to making a correction equation for quantitatively determining ammonia in the mixed gas produced by thermal decomposition of metal amides.

[0019] Furthermore, the setting of the preset thermogravimetric analysis program includes: continuously introducing helium at a flow rate of 30 mL / min, and heating from room temperature to 350° C. at a heating rate of 8° C. / min.

[0020] Furthermore, the settings of the preset gas chromatography-mass spectrometry analysis program include: the injection port temperature is set to 200°C, the split ratio is 2:1, the gas column oven is first heated from 50°C to 200°C at a rate of 10°C / min, the chromatographic column is a styrene-divinylbenzene copolymer gas chromatography column equipped with an integrated particle trap, the column flow rate is 2mL / min, the mass spectrometer is an EI source, the ionization energy is 70eV, the ion source temperature is 230°C, the MS quadrupole temperature is 150°C, the full scan mode, and the scan range is 10 m / z -350m / z.

[0021] The beneficial effects of the present invention are as follows: the performance testing method of the metal amide hydrogen storage material of the present invention takes a short time, and only 1 to 3 hours are required to analyze the ammonia release of the metal amide sample at different temperatures. The reversibility of hydrogen absorption and desorption of the metal amide hydrogen storage material can be judged from another perspective. Only 20 mg to 100 mg of sample is required for one test to obtain rich data information. In addition to being able to preliminarily judge the reversibility of the material, it is also conducive to further research on the material in the future.

[0022] Other features and advantages of the present application will be described in the following description, and partly become apparent from the description, or understood by practicing the present application. The purpose and other advantages of the present application can be realized and obtained by the structures particularly pointed out in the written description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a connection diagram of the analytical instrument provided in the embodiment of the present application.

[0024] Figure 2 This is the thermogravimetric analysis result of a certain metal amide.

[0025] Figure 3 is the calibration curve prepared using the standard substance in Example 1.

[0026] Figure 4 This is a graph showing the thermogravimetric analysis results of the sample from Example 1.

[0027] Figure 5 It is a graph of the peak area of ​​the mass spectrometry signal of ammonia corresponding to different weight loss temperature points of the sample in Example 1.

[0028] Figure 6 This is the calibration curve prepared using the standard substance in Example 2.

[0029] Figure 7 This is the thermogravimetric analysis result of the sample in Example 2.

[0030] Figure 8 It is a peak area diagram of ammonia mass spectrometry signal corresponding to different weight loss temperature points of the sample in Example 2. Figure numerals: 1, thermogravimetric analyzer; 2, gas chromatography-mass spectrometry; 3, gas sample storage; 31, first pipeline; 32, second pipeline; 33, storage tank. DETAILED DESCRIPTION

[0031] The principle of solid-state hydrogen storage is the "adsorption" and "desorption" of hydrogen by metal hydrides. When hydrogen comes into contact with these metals under a certain pressure and temperature, it forms chemical bonds with the metals to generate hydrides, and the hydrogen is "solidified" in the metal lattice; by heating or reducing pressure, the hydrogen stored in the material will be released and restored to gaseous hydrogen. However, adsorption and desorption are not 100% reversible. When researchers develop a new hydrogen storage material, they need to evaluate its various properties, among which the evaluation of the reversibility of hydrogen absorption and desorption is very important.

[0032] As a type of solid-state hydrogen storage material, metal amide composite system hydrogen storage materials release ammonia as a byproduct during the dehydrogenation process. Most of the ammonia is generated from the self-decomposition of metal amides, and the higher the temperature, the greater the amount of ammonia released. After 270 cycles of hydrogen absorption and desorption, there will be a 25% decline in hydrogen absorption and desorption capacity, of which about 1 / 3 is due to the release of ammonia. [1] , thereby reducing the reversibility of hydrogen addition and desorption of the material; this scheme reversely infers from this conclusion that measuring the amount of ammonia released can quickly determine the reversibility of hydrogen addition and desorption of metal amide hydrogen storage materials from another perspective.

[0033] It should be noted that the test results of this application are not completely equivalent to the traditional hydrogen absorption and desorption cycle test, but they can indeed preliminarily determine the reversibility of hydrogen absorption and desorption of metal amide hydrogen storage materials. It can be used as a preliminary screening method to reduce the time required to detect various parameters in the process of developing new materials. It can not only make a preliminary judgment on the reversibility of hydrogen absorption and desorption of the material, but also generate a lot of data information related to the thermal decomposition of the material, which is helpful for the evaluation of other items of the material.

[0034] The ammonia intermediate reaction mechanism believes that ammonia is an intermediate released by the decomposition of metal amides during heating, and then reacts rapidly with metal hydrides to generate hydrogen. Determining the amount of ammonia released can assist in proving the reaction mechanism of metal amides.

[0035] In addition, hydrogen fuel cells are key components that affect the performance of motor vehicles. Solid-state hydrogen storage materials provide hydrogen for fuel cells, and hydrogen is electrochemically oxidized to generate electricity. The trace amount of ammonia contained in hydrogen can affect the performance of the battery and even poison the battery. It is generally understood that ammonia reacts with hydrogen ions (H + ) reacts to form ammonium ions (NH4 + ) leads to a decrease in the conductivity of the electrolyte membrane, which has an irreversible impact on battery performance. In view of the significant poisoning effect of ammonia, the International Fuel Cell Standardization Organization has set its standard concentration in hydrogen at 0.1 parts per million (ppm). How to reduce ammonia release is particularly critical in the research of metal amide composite system hydrogen storage materials.

[0036] This application can not only make a preliminary judgment on the reversibility of hydrogen absorption and desorption of the material, but also help to study the reaction mechanism of metal amides and monitor the adverse effects of metal amides on fuel cells.

[0037] If the PCT curve and the hydrogen absorption and desorption kinetic curve cyclic test are carried out in accordance with GB / T 33291-2016 "Pressure-Composition-Isotherm (PCT) Test Method for Reversible Hydrogen Absorption and Desorption of Hydride", only the hydrogen absorption and desorption capacity can be compared, and the type of gas produced and the amount of ammonia released cannot be directly derived, which is not convenient for the subsequent research on the reaction mechanism of metal amide hydrogen storage materials.

[0038] If we refer to GB / T 43361-2023 "Confirmation of the analysis method of hydrogen fuel for proton exchange membrane fuel cells for road vehicles with gas analysis", the commonly used methods for testing ammonia in hydrogen are Fourier infrared spectroscopy and continuous wave cavity ring-down spectroscopy, and the detection methods for other impurity gases are gas chromatography. Gas chromatography requires the collection of more than 0.1L of gas released by hydrogen storage materials, while Fourier infrared spectroscopy and continuous wave cavity ring-down spectroscopy require the collection of more than 0.5L of gas. In order to avoid air interference during gas sampling, the entire system will be cleaned with the gas to be tested, so more gas samples are actually needed. If you want to explore the purity of hydrogen produced by the material under different conditions, you need to collect gas repeatedly. In summary, a single gas production test will consume a lot of material and labor costs. In order to save costs, general material research will synthesize a small number of samples for exploration, and it is difficult to evaluate the gas production purity of hydrogen storage materials using the above method.

[0039] In view of the above problems, the metal amide hydrogen storage material performance testing method of the present application is implemented according to the following steps: S1: Take a sample and perform thermogravimetric analysis according to the preset thermogravimetric analysis program, and collect the associated gas from the thermogravimetric analyzer at the weight loss temperature point.

[0040] S2: The associated gases collected at multiple weight loss temperature points are respectively transported to a gas chromatography-mass spectrometer, and analyzed according to a preset gas chromatography-mass spectrometry analysis program to generate a sample thermal decomposition gas spectrum for the associated gases corresponding to each weight loss temperature point.

[0041] S3: Select the thermal decomposition gas spectrum of the sample with ammonia produced, extract the ion chromatogram with a mass-to-charge ratio of 17 from it, calculate the first peak area of ​​the ammonia mass spectrum signal at the corresponding weight loss temperature point, and calculate the ammonia release amount.

[0042] This method can be achieved by Figure 1 The thermogravimetric analyzer 1 is connected to the inlet of the gas sample storage 3 through the first pipeline 31, and the outlet of the gas sample storage 3 is connected to the gas chromatography-mass spectrometer 2 ( Figure 1 GC stands for gas chromatography, and MS stands for mass spectrometry). The first pipeline 31 and the second pipeline 32 can be heating pipelines, the temperature of the heating pipelines is adjustable, and the outside is wrapped with insulation materials. The temperature of the gas sample storage 3 and the heating pipeline is adjusted to 200° C., and the temperature is constant.

[0043] Accordingly, the step of collecting associated gas from the thermogravimetric analyzer in step S1 includes: The associated gas in the thermogravimetric analyzer is transported to the gas sample storage device through the first pipeline, and the associated gas collected at different weight loss temperature points is stored in different partitions.

[0044] The step of conveying the associated gases collected at multiple weightlessness temperature points to the gas chromatograph-mass spectrometer in step S2 includes conveying the associated gases in multiple partitions to the gas chromatograph-mass spectrometer in batches via the second pipeline.

[0045] The above partitions can be multiple independent storage tanks 33 arranged in the gas sample storage 3. The sample amount required for one test of the thermogravimetric analyzer and gas chromatograph-gas spectrometer analysis technology is 20 mg to 100 mg. The gas produced by the thermogravimetric analyzer will be stored in the gas sample storage, and each storage tank collects and stores 250 μL of gas. A small amount of sample can be used to obtain rich data information, which is more cost-effective than conventional hydrogen purity analysis and testing.

[0046] Specifically, the preset thermogravimetric analysis program includes: continuously introducing helium at a flow rate of 30 mL / min, and heating from room temperature to 350° C. at a heating rate of 8° C. / min. The subsequent Examples 1 and 2 were both subjected to thermogravimetric analysis according to this program.

[0047] The preset gas chromatography-mass spectrometry analysis program settings include: selecting a highly inert injection port, setting the injection port temperature to 200°C, a split ratio of 2:1, the gas phase column oven is first heated from 50°C to 200°C at a rate of 10°C / min, the chromatographic column is a styrene-divinylbenzene copolymer gas chromatography column (30m*0.32mm*20μm) equipped with an integrated particle trap, the column flow rate is 2mL / min, the mass spectrometer selects an EI high-sensitivity inert ion source, the ionization energy is 70eV, the ion source temperature is 230°C, the MS quadrupole temperature is 150°C, the full scan mode, and the scan range is 10 m / z-350m / z. Subsequent Examples 1 and 2 are all subjected to gas chromatography-mass spectrometry analysis according to this program.

[0048] The weight loss temperature point refers to a temperature point set by the tester, and the sample will thermally decompose at this temperature. For example, if a sample will thermally decompose above 120°C, 125°C, 150°C, etc. can be set as the weight loss temperature point. Accordingly, during the process of the sample heating up from room temperature to 130°C, the associated gas is collected in step S1, and only the associated gas at the moment of reaching 125°C is collected; during the process of the temperature continuing to rise to 160°C, only the associated gas at the moment of reaching 150°C is collected.

[0049] When faced with newly synthesized metal amides, it may be impossible to predict their decomposition temperature, but preliminary experiments can be performed to understand their thermal decomposition characteristics.

[0050] For example, take two parts of metal amide type hydrogen storage material; The first material is subjected to thermogravimetric analysis according to a preset thermogravimetric analysis program to obtain a TG curve and a DSC curve. The temperature at which the TG curve begins to lose weight is taken as the starting point, and the temperature at which the exothermic process of the DSC curve ends is taken as the end point, to obtain the temperature range of weight loss before decomposition of the sample; Select multiple weight loss temperature points within the weight loss temperature range before decomposition; The second material was subjected to thermogravimetric analysis according to a preset thermogravimetric analysis program, and associated gas was collected from the thermogravimetric analyzer at multiple weight loss temperature points.

[0051] The selection of the weight loss temperature point should try to cover the entire range of the metal amide continuous weight loss with increasing temperature. Therefore, preferably, the selection point requirements meet: The extreme low and extreme high values ​​of the weight loss temperature point span more than 60% of the preset temperature range and span the continuous endothermic-exothermic peaks of the DSC curve; The preset temperature range starts at the temperature where the sample starts to lose weight and ends at the end temperature of the continuous endothermic-exothermic peak in the DSC curve. The following example is used to illustrate the point selection requirements.

[0052] The inventor has synthesized a metal amide in the project, and the results of the thermogravimetric analysis are as follows: Figure 2 shown. Figure 2 In the figure, the top one is the TG (thermogravimetric) curve, and the bottom one is the DSC curve. The horizontal axes of the TG and DSC curves are both heating time and aligned, but the vertical axes are different. The vertical axis of the TG curve is the residual weight of the sample (unit: mg), and the vertical axis of the DSC curve is the heat flow rate (unit: mW). In this test, the starting room temperature is 30°C. The time on the horizontal axis multiplied by the heating rate of 8°C / min in the preset thermogravimetric analysis program plus the starting room temperature is the corresponding heating temperature. Figure 2 It can be seen from the TG curve that the sample starts to lose weight at 79°C. Metal amide hydrogen storage materials have a very obvious feature when doing thermogravimetric analysis. The DSC curve will have a sharp endothermic peak, followed by an exothermic peak, such as the two peaks of the sample at 23.5min~31min. The end of the exothermic peak is used as the maximum value of the weight loss temperature point that can be set.

[0053] According to the definition of the preset temperature range, the starting point of the preset temperature range is 79°C and the end point is 278°C. According to the selection point requirements, the selection point of the weight loss temperature point can fall within the range of 79°C~278°C, 120°C~278°C, 158°C~278°C, etc. Although 79°C~200°C spans more than 60% of the preset temperature range, it does not span the continuous endothermic-exothermic peak of the DSC curve, which does not meet the selection point requirements. Next, taking the selection point range of 120°C~278°C as an example, 10 weight loss temperature points can be selected, such as 120°C, 130°C, 140°C, 150°C, 180°C, 200°C, 220°C, 240°C, 260°C, and 278°C. Note that the weight loss temperature points may not be equally spaced. Preferably, more dense weight loss temperature points can be set at the continuous endothermic-exothermic peak of the DSC curve.

[0054] In step S3, the step of calculating the amount of ammonia released includes: Substitute the first peak area into the calibration equation to obtain the ammonia release amount.

[0055] The steps of obtaining the correction equation include: S01: Standard substances of different masses are divided into groups and subjected to thermogravimetric analysis according to a preset thermogravimetric analysis program, and multiple groups of product gases are collected from the thermogravimetric analyzer.

[0056] S02: The product gases of each group are respectively transported to a gas chromatography-mass spectrometer, and analyzed according to a preset gas chromatography-mass spectrometry analysis program to obtain a thermal decomposition gas spectrum of the standard substance, which is compared with the standard spectrum library to obtain the retention time of the chromatographic peak where ammonia is located, and the ion chromatogram with a mass-to-charge ratio of 17 is extracted to obtain the second peak area of ​​the ammonia mass spectrometry signal.

[0057] S03: Taking the theoretical ammonia mass produced by thermal decomposition of the standard as the independent variable and the second peak area as the dependent variable, the least squares method is used to fit the linear regression equation to obtain the correction equation.

[0058] For example, ammonium bicarbonate (20 mg, 40 mg, 60 mg, 80 mg, high purity or above) of gradient mass is placed in the sample tank of the thermogravimetric analyzer, and the above thermogravimetric analysis program is run to obtain the chromatogram and mass spectrum of the thermal decomposition gas of ammonium bicarbonate. The chromatographic peak position RT (retention time) of ammonia is obtained by comparison with the NIST spectral library, and the ion chromatogram with m / z of 17 is extracted to obtain the mass spectrum signal peak area of ​​ammonia. The mass of ammonia (4.3081 mg, 8.6162 mg, 12.9244 mg, 17.2325 mg, which are the theoretical ammonia yields when 20 mg, 40 mg, 60 mg, and 80 mg of ammonium bicarbonate are thermally decomposed) is used as the horizontal coordinate, and the peak area of ​​the mass spectrum signal of ammonia is used as the vertical coordinate, and the least squares method is used to fit the linear regression equation.

[0059] In step S3, the step of selecting the thermal decomposition gas spectrum of the sample with ammonia generated comprises: The retention time of the ammonia peak in the thermal decomposition gas spectrum of the standard is compared to select the thermal decomposition gas spectrum of the sample producing ammonia.

[0060] The complete step S3 may be, for example: (1) using the NIST spectral library to search and qualitatively analyze the composition information of the cracking gas; (2) comparing the retention time of the ammonia peak in the chromatogram of the sample and the ammonium bicarbonate thermal decomposition gas to determine whether ammonia is generated; (3) extracting the ion chromatogram of the gas sample with m / z 17 to obtain the mass spectrum signal peak area of ​​ammonia, and substituting it into the calibration equation to obtain the amount of ammonia released.

[0061] Example 1 Calibration of ammonia: ammonium bicarbonate of gradient mass (26.76 mg, 45.86 mg, 60.65 mg, 79.18 mg) was placed in the sample tank of the thermogravimetric analyzer, and the thermal decomposition gas spectrum of the standard was obtained after thermogravimetric analysis and gas chromatography-mass spectrometry analysis. The chromatographic peak position of ammonia in the thermal decomposition gas spectrum of the standard was obtained by comparison with the NIST spectrum library, and the retention time of the chromatographic peak position of ammonia was obtained (roughly starting at 3.2 min and ending at 3.7 min). The ion chromatogram with a mass-to-charge ratio of 17 in the chromatographic peak position (the chromatographic peak position of ammonia in the thermal decomposition gas spectrum of the standard) was extracted to obtain the ammonia mass spectrum signal peak area (the second peak area, which is generated by the analysis program of the gas chromatography-mass spectrometry). According to the second peak area and the theoretical ammonia yield, the calibration equation y=1371119.19x-7760215.02 was obtained by fitting. The fitting curve is shown as follows: Figure 3 shown.

[0062] Test of hydrogen storage material sample (doped metal amide): Weigh 48.30 mg of sample into the sample tank of thermogravimetric analyzer, run the program of thermogravimetric analyzer, and obtain the thermogravimetric curve of the material, such as Figure 4 To observe the data more intuitively, Figure 2 different, Figure 4 The horizontal axes of the TG curve and the DSC curve are still aligned, but the meaning of the horizontal axis is changed to the heating temperature; the vertical axis of the TG curve is changed to the percentage of the remaining weight of the sample relative to the initial weight; the vertical axis unit of the DSC curve is changed to watt / gram.

[0063] The gases released by the thermogravimetric analyzer were collected at 60°C, 100°C, 110°C, 120°C, 160°C, 180°C, 185°C, 190°C, 200°C, 210°C, 220°C, 230°C and 240°C into a gas sample storage device, and then injected into a gas chromatography-mass spectrometer for analysis in sequence to obtain 13 gas sample chromatograms and mass spectra, all of which had chromatographic peaks at 3.2min-3.7min. It was determined that ammonia was generated at all 13 weightlessness temperatures, and the part with a mass-to-charge ratio of 17 was extracted to obtain the mass spectrometry signal peak area (response value) of ammonia. The 13 peak areas were plotted on the same graph, as shown in Figure 2. Figure 5 As shown, Figure 5 The horizontal axis is temperature.

[0064] Finally, the peak area of ​​the ammonia mass spectrometry signal was substituted into the calibration curve to obtain the ammonia yield. Taking 230°C as an example, the ammonia peak area of ​​the gas sample was 147659.18, and after substituting it into the fitting equation, the total ammonia release was 5.77 mg.

[0065] Example 2 Calibration of ammonia: ammonium bicarbonate of gradient mass (21.33 mg, 40.16 mg, 58.77 mg, 79.58 mg) was placed in the sample tank of the thermogravimetric analyzer, and the thermal decomposition gas spectrum of the standard was obtained after thermogravimetric analysis and gas chromatography-mass spectrometry analysis. The chromatographic peak position of ammonia in the thermal decomposition gas spectrum of the standard was obtained by comparison with the NIST spectrum library, and the retention time of the chromatographic peak position of ammonia was obtained. The ion chromatogram with a mass-to-charge ratio of 17 in the chromatographic peak position was extracted to obtain the peak area of ​​ammonia mass spectrum signal. According to the second peak area and the theoretical ammonia yield, the calibration equation y=1320692.901x-5185040.32 was obtained by fitting. The fitting curve is shown as follows: Figure 6 shown.

[0066] Another test of hydrogen storage material sample (doped metal amide): 36.17 mg of the sample was weighed into the sample tank of the thermogravimetric analyzer, and the program of the thermogravimetric analyzer was run to obtain the thermogravimetric curve of the material, such as Figure 7 shown.

[0067] The gases released by the thermogravimetric analyzer were collected at 100°C, 110°C, 120°C, 160°C, 180°C, 200°C, 220°C, 230°C, and 240°C into a gas sample storage device, and then injected into a gas chromatography-mass spectrometer for analysis in sequence to obtain 9 gas sample chromatograms and mass spectra, confirming that all ammonia was generated. The part with a mass-to-charge ratio of 17 was extracted to obtain the mass spectrometry signal peak area of ​​ammonia, and the 9 peak areas were plotted on the same curve, as shown in FIG. Figure 8 As shown, Figure 8 The horizontal axis is temperature.

[0068] Finally, the peak area of ​​the ammonia mass spectrometry signal was substituted into the calibration curve to obtain the ammonia yield. Taking 180°C as an example, the ammonia peak area of ​​the gas sample is 169652.95, and after substituting it into the equation, the total ammonia release is 4.05 mg.

[0069] This application uses the amount of ammonia released to evaluate the reversibility of hydrogen addition and desorption of metal amide hydrogen storage materials, which is different from the evaluation dimension of the conventional method of comparing the hydrogen absorption and desorption capacity under different cycles after multiple cycles of hydrogen absorption and desorption. The principle of this application being able to quickly and preliminarily determine the reversibility of hydrogen addition and desorption of metal amide hydrogen storage materials is that metal amide hydrogen storage materials release hydrogen when heated, and ammonia is an intermediate gas in the reaction process during normal operation and will not escape easily. The chemical formula of the ammonia intermediate mechanism is as follows:

[0070] Ammonia is an intermediate product and will not escape. Normally, it should be immediately converted into other nitrogen-hydrogen compounds and retained inside the material. If ammonia escape is detected, it means that the material will be damaged when working at this temperature, which will directly lead to a reduction in the amount of material participating in hydrogen storage next time. From this, the reversibility of hydrogen absorption and desorption of the material can be judged. Thermogravimetric analyzer and gas chromatography-mass spectrometry analyzer take about 1 hour to 3 hours to analyze metal amide samples. After the analysis is completed, the amount of ammonia released by the material at different temperatures can be obtained. The amount of ammonia released can be used to screen materials with better reversibility of hydrogen addition and desorption. Comparative cycle test of hydrogen absorption and desorption kinetic curve test saves more time.

[0071] The combination of the thermogravimetric analyzer, gas chromatography-mass spectrometry and gas sample storage device of the present application, as well as various preset condition parameters, is specifically used to test the release of ammonia from metal amide hydrogen storage materials. It can not only quickly and preliminarily determine the reversibility of hydrogen addition and desorption from metal amide hydrogen storage materials, but also simultaneously obtain multiple sets of data such as thermal stability information of the material to be tested, precipitation time and precipitation intensity of pyrolysis components, component information of pyrolysis components, pyrolysis gas content, etc., providing richer information on the complex thermochemical reactions of the material, which is convenient for subsequent research on the change mechanism of the material.

[0072] In the description of this specification, the description with reference to the terms "one embodiment", "certain embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0073] The above is a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the present invention. These improvements and modifications are also considered to be within the scope of protection of the present invention.

[0074] References [1]WF Luo, J. Wang, K. Stewart, M. Clift and K. Gross. Li-Mg-NH:Recent investigations and development. Journal of Alloys and Compounds,2007,446:336-341.

Claims

1. A method for testing the performance of metal amide hydrogen storage materials. It is characterized in that The following steps are involved: Take a sample and perform thermogravimetric analysis according to a preset thermogravimetric analysis program, and collect associated gas from the thermogravimetric analyzer at the weight loss temperature point; The associated gases collected at the plurality of weight loss temperature points are respectively transported to a gas chromatography-mass spectrometer, and analyzed according to a preset gas chromatography-mass spectrometry analysis program, and a sample thermal decomposition gas spectrum is generated for the associated gases corresponding to each weight loss temperature point; The thermal decomposition gas spectrum of the sample with ammonia produced is selected, and the ion chromatogram with a mass-to-charge ratio of 17 is extracted therefrom. The first peak area of ​​the ammonia mass spectrum signal at the corresponding weightlessness temperature point is calculated, and the ammonia release amount is calculated.

2. The method for testing the performance of metal amide hydrogen storage materials according to claim 1, It is characterized in that The step of collecting associated gas from the thermogravimetric analyzer comprises: The associated gas in the thermogravimetric analyzer is transported to a gas sample storage device via a first pipeline, and the associated gas collected at different weight loss temperature points is stored in different partitions; The step of respectively transporting the associated gases collected at the plurality of weightlessness temperature points to a gas chromatography-mass spectrometer comprises: The associated gas in the plurality of partitions is transported in batches to a gas chromatograph-mass spectrometer via a second pipeline.

3. The method for testing the performance of metal amide hydrogen storage materials according to claim 2, It is characterized in that The first pipeline, the second pipeline and the gas sample storage are all kept at 200°C.

4. The method for testing the performance of metal amide hydrogen storage materials according to claim 1, It is characterized in that The step of taking samples for thermogravimetric analysis according to a preset thermogravimetric analysis program and collecting associated gas from the thermogravimetric analyzer at the weight loss temperature point comprises: Take two portions of metal amide type hydrogen storage material; The first material is subjected to thermogravimetric analysis according to the preset thermogravimetric analysis program to obtain a TG curve and a DSC curve, and the temperature at which the TG curve begins to lose weight is taken as the starting point, and the temperature at which the exothermic process of the DSC curve ends is taken as the end point, to obtain the temperature range of weight loss before decomposition of the sample; Selecting a plurality of weight loss temperature points within the weight loss temperature range before decomposition; The second material is used as the sample, and a thermogravimetric analysis is performed according to the preset thermogravimetric analysis program, and associated gas is collected from the thermogravimetric analyzer at multiple weight loss temperature points.

5. The method for testing the performance of metal amide hydrogen storage materials according to claim 4, It is characterized in that In the step of selecting a plurality of weight loss temperature points within the weight loss temperature range before decomposition, the selection requirements satisfy: The extreme low value and the extreme high value of the weight loss temperature point span more than 60% of the preset temperature range and span the continuous endothermic-exothermic peak of the DSC curve; The preset temperature range starts at the temperature at which the sample starts to lose weight and ends at the end temperature of the continuous endothermic-exothermic peak in the DSC curve.

6. The method for testing the performance of metal amide hydrogen storage materials according to claim 1, It is characterized in that The step of calculating the ammonia release amount comprises: Substituting the first peak area into a calibration equation to obtain the ammonia release amount; The step of obtaining the correction equation comprises: Taking standard substances of different masses into groups and performing thermogravimetric analysis according to the preset thermogravimetric analysis program, collecting multiple groups of product gases from the thermogravimetric analyzer; The product gases of each group are respectively transported to a gas chromatography-mass spectrometer, and analyzed according to a preset gas chromatography-mass spectrometry analysis program to obtain a thermal decomposition gas spectrum of a standard substance, and compared with a standard spectrum library to obtain a chromatographic peak position of ammonia in the thermal decomposition gas spectrum of the standard substance, and an ion chromatogram with a mass-to-charge ratio of 17 is extracted to obtain a second peak area of ​​ammonia mass spectrum signal; The theoretical ammonia mass generated by the thermal decomposition of the standard substance is used as the independent variable, the second peak area is used as the dependent variable, and the least square method is used to perform linear regression equation fitting to obtain the correction equation.

7. The method for testing the performance of metal amide hydrogen storage materials according to claim 6, It is characterized in that The step of selecting the sample thermal decomposition gas spectrum containing ammonia gas comprises: According to the retention time of the chromatographic peak position of ammonia in the thermal decomposition gas spectrum of the standard substance, the thermal decomposition gas spectrum of the sample in which ammonia is produced is selected.

8. The method for testing the performance of metal amide hydrogen storage materials according to claim 6, It is characterized in that The steps also include: The thermal decomposition gas spectrum of the sample is compared with the standard spectrum library to determine the gas components decomposed by the sample at the weightlessness temperature point.

9. The method for testing the performance of metal amide hydrogen storage materials according to claim 6, It is characterized in that The standard was ammonium bicarbonate.

10. The method for testing the performance of metal amide hydrogen storage materials according to claim 1, It is characterized in that The preset thermogravimetric analysis program settings include: continuously introducing helium at a flow rate of 30 mL / min, and heating from room temperature to 350° C. at a heating rate of 8° C. / min; The settings of the preset gas chromatography-mass spectrometry analysis program include: the injection port temperature is set to 200°C, the split ratio is 2:1, the gas column oven is first heated from 50°C to 200°C at a rate of 10°C / min, the chromatographic column uses a styrene-divinylbenzene copolymer gas chromatography column with an integrated particle trap, the column flow rate is 2mL / min, the mass spectrometer uses an EI source, the ionization energy is 70eV, the ion source temperature is 230°C, the MS quadrupole temperature is 150°C, the full scan mode, and the scan range is 10 m / z -350m / z.

Citation Information

Patent Citations

  • Method for preparing a composite hydrogen storage material of borohydride and magnesium chloride ammonia complex

    CN101519185A

  • Method for measuring element contents by using thermogravimetric-mass spectrometry

    CN109696375A

  • Measuring material quantity determination method, and gas chromatograph mass spectrograph using it

    JP2009257961A

Cited By

  • Method for analyzing and testing outgassing performance of sealing material and application thereof

    CN122487173A