Negative pole piece capable of improving double-layer coating abnormity as well as preparation method and application of negative pole piece
By adding an additional coating area to the double coating of silicon negative electrode material of lithium-ion batteries and cleaning with a laser etching machine, the problem of irregular pattern of the coating layer is solved, the battery performance and cycle stability are improved, and the pole-piece tape is avoided The phenomenon has achieved high energy density and stability.
Patent Information
- Application Number
- CN202411094176.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
During the double coating process of silicon negative electrode material of lithium-ion batteries, the mutual dissolution of the upper and lower slurries lead to irregular patterns in the coating layer, affecting the battery performance and cycle stability, and easily lead to abnormal pole thickness and strip breakage. Impact production efficiency.
By adding additional coating areas to the head and tail of the coating layer and laser cleaning with a laser etching machine, the abnormal areas are thoroughly removed to ensure density uniformity and kinetic properties of the coating layer.
It effectively improves the double-layer coating effect of silicon negative electrode sheets, avoids the phenomenon of electrode segmentation, improves battery performance and cycle stability, and ensures the high energy density and long-term use stability of lithium-ion batteries.
Smart Images

Figure CN119008831A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-ion batteries, and in particular to a negative electrode sheet for improving double-layer coating abnormality, and a preparation method and application thereof. Background Art
[0002] Competition in the lithium-ion battery 3C consumer market is becoming increasingly fierce, and the energy density of lithium-ion batteries is also increasing. Graphite is a commonly used negative electrode material in lithium-ion batteries. The theoretical specific capacity of graphite negative electrode materials is about 372mAh / g. As the industry matures, the actual specific capacity of graphite negative electrode materials has reached 340-360mAh / g, which is close to the theoretical capacity and has little room for improvement. The graphite negative electrode system using a single-layer coating process can no longer meet the high energy density requirements of clients.
[0003] Silicon negative electrode materials are regarded as ideal candidates for the next generation of high energy density lithium-ion battery negative electrode materials. The theoretical specific capacity of silicon negative electrode materials is as high as 4200mAh / g, far exceeding the 372mAh / g of graphite negative electrode materials, and has great commercial application potential. Researchers have begun to use high gram capacity silicon negative electrode materials with negative electrode double-layer coating technology, that is, the surface slurry uses small-particle fast-charging active materials, and the bottom slurry uses large-particle high-compactness active materials, which can achieve stratified control of porosity, reduce surface overpotential, and greatly improve the working performance of lithium batteries. In the double-layer coating process of silicon negative electrode materials, the upper and lower layers of slurry need to be coated on both sides at the same time; however, there is a certain compatibility between the upper and lower layers of slurry. At the start and end of coating, with the change of flow ratio and momentum, the two slurries are easily miscible, resulting in stripes extending along the width direction at the head and tail parts of the coating layer, showing an irregular pattern; since the upper and lower slurries of the irregular pattern part are miscible, the electrode dynamics here will be insufficient, affecting the battery performance and long-term cycle stability of the battery; and the density of the irregular pattern part is uneven, the thickness of the electrode will be abnormal after thinning, which may easily lead to over-rolling of the electrode during the rolling process or even the phenomenon of electrode breakage, seriously affecting the production progress and efficiency; therefore, it is necessary to provide a solution that can improve the poor double-layer coating effect of the negative electrode to solve the above problems. Summary of the invention
[0004] In view of the above problems existing in the prior art, the object of the present invention is to provide a negative electrode plate with improved double-layer coating abnormality, and a preparation method and application thereof.
[0005] To achieve the above object, the present invention adopts the following technical solutions:
[0006] The present invention provides a method for preparing a negative electrode sheet with improved double-layer coating abnormality, comprising the following steps:
[0007] Double-layer coating is performed on both sides of the negative electrode current collector, wherein the coating areas on both sides of the negative electrode current collector include an effective coating area and two additional coating areas respectively located at the head and tail ends of the effective coating area;
[0008] The additional coating area is laser cleaned by using a laser etching machine to expose the surface of the negative electrode current collector to obtain a negative electrode plate.
[0009] In some embodiments, the step of laser cleaning the additional coating area with a laser etching machine to expose the surface of the negative electrode current collector to obtain the negative electrode plate includes:
[0010] Cleaning the surface coating of the additional coating area once with a laser etching machine, and rolling up the negative electrode current collector after the cleaning is completed;
[0011] Unwinding the negative electrode current collector, and performing secondary cleaning on the bottom coating of the additional coating area using a laser etching machine;
[0012] The cleaned additional coating area located at the tail of the coating area on the negative electrode current collector is cut off to obtain a negative electrode plate.
[0013] In some embodiments, the total laser cleaning depth of the additional coating area by the laser etcher is greater than the total thickness of the top coating and the bottom coating.
[0014] In some embodiments, the area of the laser cleaning is equal to the area of the additional coating area; the length of the additional coating area is 3-15 mm, and the width of the additional coating area is equal to the width of the effective coating area.
[0015] In some embodiments, the mass ratio of the active material in the bottom coating layer to the active material in the top coating layer is 60-85%:15-40%;
[0016] The active material used in the bottom coating is a mixture of large-particle high-density graphite and silicon-carbon material, and the active material used in the surface coating is small-particle fast-filling graphite;
[0017] The mass ratio of the large-particle high-density graphite to the silicon-carbon material in the mixture of the large-particle high-density graphite and the silicon-carbon material is 75-95%:5-25%;
[0018] The single-sided surface density of the bottom coating is ≥36g / m 2 ; The single-sided surface density of the surface coating is ≥13g / m 2 .
[0019] In some embodiments, the laser power of the first cleaning is 300-1000W; the laser power of the second cleaning is 800-3000W; the diameter of the laser spot used in the laser cleaning is 0.02-1.0mm; the laser pulse frequency used in the laser cleaning is 0.1-800Hz.
[0020] In some embodiments, both sides of the negative electrode current collector include a long film surface and a short film surface; the length of the effective coating area of the short film surface is smaller than the length of the effective coating area of the long film surface, and the tail of the effective coating area of the short film surface is aligned with the tail of the effective coating area of the long film surface; the lengths of the two additional coating areas at the head and tail of the coating area of the short film surface are equal to the lengths of the two additional coating areas at the head and tail of the coating area of the long film surface.
[0021] In some embodiments, in the one cleaning, the laser cleaning power at the tail of the short film surface coating area is P1, the laser cleaning power at the head of the short film surface coating area is P2, the laser cleaning power at the tail of the long film surface coating area is P3, and the laser cleaning power at the head of the long film surface coating area is P4; wherein P1=P2=P3=P4;
[0022] In the secondary cleaning, the laser cleaning power at the tail of the short film surface coating area is P5, the laser cleaning power at the head of the short film surface coating area is P6, the laser cleaning power at the tail of the long film surface coating area is P7, and the laser cleaning power at the head of the long film surface coating area is P8; wherein, P5=P6=P7=P8;
[0023] The laser spot diameter used for laser cleaning of the tail of the short film surface coating area is D1, the laser spot diameter used for laser cleaning of the head of the short film surface coating area is D2, the laser spot diameter used for laser cleaning of the tail of the long film surface coating area is D3, and the laser spot diameter used for laser cleaning of the head of the long film surface coating area is D4; wherein, D1=D2=D3=D4;
[0024] The pulse frequency used for laser cleaning the tail of the short film surface coating area is f1, the pulse frequency used for laser cleaning the head of the short film surface coating area is f2, the pulse frequency used for laser cleaning the tail of the long film surface coating area is f3, the pulse frequency used for laser cleaning the head of the long film surface coating area is f4; wherein, f1=f2=f3=f4.
[0025] The present invention also provides a negative electrode plate, which is obtained by cleaning and removing local areas at the head and tail of the coating layer in the double-layer coating by a laser etching machine.
[0026] The present invention further provides a lithium-ion battery, comprising a positive electrode sheet and the above-mentioned negative electrode sheet.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] In the present invention, in the process of preparing the negative electrode pole piece, a certain length is additionally added to the head and tail of the coating layer under the originally required coating length, and the length of the negative electrode pole piece for coating is also increased accordingly; the originally required coating length part belongs to the effective coating area, and the added length is regarded as the additional coating area; since the additional coating area is arranged at the head and tail ends of the coating range, the additional coating area will locally show striped patterns due to the mutual dissolution of the upper and lower slurries of the double-layer coating; the present invention completely removes the entire additional coating area through continuous laser cleaning of a laser etching machine, and the coating on the surface of the pole piece will be converted into plasma under high-power laser etching, directly eliminating such irregular pattern areas that are prone to abnormal thickness thinning, excessive rolling and affect the dynamic properties of the pole piece; the present invention improves the poor coating effect of the silicon negative electrode pole piece in the double-layer coating process, avoids the phenomenon of pole piece breakage that may occur in the subsequent pole piece processing process, and improves the quality and efficiency of the pole piece output, thereby ensuring the performance and cycle stability of the lithium-ion battery prepared by the negative electrode pole piece. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Schematic diagram of the CNT double-sided coating length of the negative electrode sheet in Example 1 of the present invention;
[0030] Figure 2 Schematic diagram of the double-layer coating structure of the negative electrode plate in Example 1 of the present invention;
[0031] Figure 3 It is a schematic diagram of the double-sided coating length of the negative electrode slurry of the negative electrode plate in Example 1 of the present invention;
[0032] Figure 4 It is a schematic plan view of the additional coating area on the long film surface of the negative electrode plate in Example 1 of the present invention;
[0033] Figure 5 It is a schematic plan view of the additional coating area on the short film surface of the negative electrode plate in Example 1 of the present invention;
[0034] Figure 6 It is a schematic plan view of the double-layer coating effect on the long film surface of the negative electrode plate in Example 1 of the present invention;
[0035] Figure 7 It is a schematic plan view of the double-layer coating effect on the short film surface of the negative electrode plate in Example 1 of the present invention;
[0036] Figure 8 This is a schematic plan view of the long film surface coating area of the negative electrode plate after laser cleaning in Example 1 of the present invention;
[0037] Fig. 9This is a schematic plan view of the short film surface coating area of the negative electrode plate after laser cleaning in Example 1 of the present invention;
[0038] Fig.10 This is a schematic diagram of the coating area length after laser cleaning of the negative electrode plate in Example 1 of the present invention;
[0039] Fig.11 It is a schematic diagram of the double-sided coating length of the positive electrode slurry of the positive electrode plate in Example 1 of the present invention;
[0040] Fig.12 This is a schematic diagram of the CNT double-sided coating length of the negative electrode sheet in Comparative Example 1 of the present invention;
[0041] Fig.13 It is a schematic diagram of the double-sided coating length of the negative electrode slurry of the negative electrode sheet in Comparative Example 1 of the present invention;
[0042] Fig.14 This is a comparison chart of the capacity retention rates of the lithium ion batteries of Example 1 and Comparative Example 1 under a voltage reduction cycle test in the test examples of the present invention;
[0043] Fig.15 It is a comparison chart of the thickness change rate of the lithium ion batteries of Example 1 and Comparative Example 1 in the test examples of the present invention under the voltage reduction cycle test. DETAILED DESCRIPTION
[0044] The embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, but are not to be construed as limiting the present invention. All other embodiments obtained by ordinary technicians in the field without creative work based on the embodiments of the present invention are within the scope of protection of the present invention.
[0045] The negative electrode sheet provided by the present invention is obtained by removing the local areas at the head and tail of the coating layer in the double-layer coating by a laser etching machine; the present invention also provides a lithium-ion battery, including a positive electrode sheet and the negative electrode sheet; the preparation method of the negative electrode sheet is as follows:
[0046] Double-layer coating is performed on both sides of the negative electrode current collector, and the coating areas on both sides of the negative electrode current collector include an effective coating area and two additional coating areas located at the head and tail ends of the effective coating area respectively;
[0047] The additional coating area is laser cleaned by using a laser etching machine to expose the surface of the negative electrode current collector to obtain a negative electrode plate.
[0048] At the beginning and end of the coating layer, the flow rate of the upper and lower layers of slurry is relatively small, the momentum changes, and the upper and lower layers of slurry with a certain degree of compatibility are easy to impact each other and dissolve each other, resulting in uneven density at the head and tail of the coating layer and irregular patterns; the effective coating area is the coating range specified by the process of the negative electrode plate. If the above-mentioned abnormal pattern appears within this range, it will cause uneven density of the plate here, resulting in abnormalities in subsequent processes such as plate thinning and rolling, and insufficient dynamics of the plate, thereby reducing battery performance; the range of abnormal pattern distribution can be slightly reduced by debugging the coating equipment, but it cannot be completely removed; for this reason, the present invention adds additional coating areas at the head and tail of the effective coating area, so that all abnormal pattern parts that appear after double-layer coating fall into the additional coating area, and then use laser to clean the additional coating area, which can completely remove the abnormal area caused by the double-layer coating process, and finally leave an effective coating area with good coating effect.
[0049] Furthermore, the step of laser cleaning the additional coating area with a laser etching machine to expose the surface of the negative electrode current collector and obtain the negative electrode sheet also includes:
[0050] Clean the surface coating of the additional coating area once with a laser etching machine, and roll up the negative electrode current collector after the cleaning is completed;
[0051] The negative electrode current collector is unwound, and the bottom coating of the additional coating area is cleaned twice using a laser etching machine;
[0052] The cleaned extra coating area at the tail of the coating area on the negative electrode current collector is cut off to obtain a negative electrode sheet.
[0053] In double-layer coating, the slurry composition of the upper and lower layers is inconsistent, and the coating density is also inconsistent. To ensure the cleaning effect, the upper and lower layers need to be laser cleaned separately; after the first cleaning and before the second cleaning, the current collector material is rewound and unwound to keep the current collector material flat and wrinkle-free to ensure the accuracy of laser cleaning; in addition, after rewinding and unwinding, the current collector material passes through a scraper, slit or roller again to improve the uneven thickness that may occur on the coating surface.
[0054] Furthermore, the total laser cleaning depth of the additional coating area by the laser etching machine is greater than the total thickness of the surface coating and the bottom coating.
[0055] In order to ensure that the coating layer on the surface of the current collector is completely cleaned, the depth of laser cleaning needs to be greater than the depth of the surface coating layer; if the surface of the current collector is also coated with a conductive agent, the depth of laser cleaning needs to be further added to the depth of the conductive agent coating layer to ensure that the conductive agent coating is also completely removed.
[0056] Furthermore, the area of laser cleaning is equal to the area of the additional coating area; the length of the additional coating area is 3-15 mm, and the width of the additional coating area is equal to the width of the effective coating area; in actual production, the length range of the additional coating area can be appropriately adjusted according to the bare cell structure after the positive and negative pole sheets are wound.
[0057] Further, the mass ratio of the active substance in the bottom coating layer to the active substance in the top coating layer is 60-85%:15-40%;
[0058] The active material used in the bottom coating is a mixture of large-particle high-density graphite and silicon-carbon material, and the active material used in the surface coating is small-particle fast-filling graphite;
[0059] The mass ratio of large-particle high-density graphite to silicon-carbon material in the mixture of large-particle high-density graphite and silicon-carbon material is 75-95%:5-25%;
[0060] The single-sided surface density of the bottom coating is ≥36g / m 2 ; Single-sided surface density of surface coating ≥13g / m 2 ; The single-sided surface density of the bottom layer and the surface coating does not include the surface density of the negative electrode collector itself.
[0061] In the double-layer coating of the present invention, the surface layer adopts small-particle fast-charging graphite with high porosity, and the bottom layer adopts a mixture of high-compacted graphite and silicon-carbon material with a high-compacted density structure, which can take into account both high energy density and super-fast charging, thereby improving battery performance.
[0062] Furthermore, the laser power for the first cleaning is 300-1000W; the laser power for the second cleaning is 800-3000W; the laser spot diameter used in laser cleaning is 0.02-1.0mm; and the laser pulse frequency used in laser cleaning is 0.1-800Hz.
[0063] Since the mass proportion of the small-particle fast-filled graphite material layer in the surface coating is relatively low, in order to reduce the power loss of laser cleaning, the surface coating is laser cleaned with a lower power; and since the mass proportion of the large-particle high-density graphite and silicon-carbon material mixture material layer in the bottom coating is relatively high, in order to ensure that the abnormal pattern area is thoroughly cleaned at one time, the surface coating is laser cleaned with a higher power.
[0064] Furthermore, both sides of the negative electrode current collector include a long film surface and a short film surface; the length of the effective coating area of the short film surface is smaller than that of the long film surface, and the tail of the effective coating area of the short film surface is aligned with the tail of the effective coating area of the long film surface; the lengths of the two additional coating areas at the head and tail of the coating area of the short film surface are equal to the lengths of the two additional coating areas at the head and tail of the coating area of the long film surface.
[0065] Furthermore, in one cleaning, the laser cleaning power at the tail of the short film surface coating area is P1, the laser cleaning power at the head of the short film surface coating area is P2, the laser cleaning power at the tail of the long film surface coating area is P3, and the laser cleaning power at the head of the long film surface coating area is P4; wherein, P1=P2=P3=P4;
[0066] In the secondary cleaning, the laser cleaning power at the tail of the short film surface coating area is P5, the laser cleaning power at the head of the short film surface coating area is P6, the laser cleaning power at the tail of the long film surface coating area is P7, and the laser cleaning power at the head of the long film surface coating area is P8; wherein, P5=P6=P7=P8;
[0067] The laser spot diameter used for laser cleaning of the tail of the short film surface coating area is D1, the laser spot diameter used for laser cleaning of the head of the short film surface coating area is D2, the laser spot diameter used for laser cleaning of the tail of the long film surface coating area is D3, and the laser spot diameter used for laser cleaning of the head of the long film surface coating area is D4; wherein, D1=D2=D3=D4;
[0068] The pulse frequency used for laser cleaning the tail of the short film surface coating area is f1, the pulse frequency used for laser cleaning the head of the short film surface coating area is f2, the pulse frequency used for laser cleaning the tail of the long film surface coating area is f3, and the pulse frequency used for laser cleaning the head of the long film surface coating area is f4; among them, f1=f2=f3=f4.
[0069] Since the thickness and surface density of the additional coating areas at the ends of the long film surface and the short film surface are similar after coating, the laser cleaning power, spot diameter and pulse frequency used in laser cleaning can generally be set to the same values. However, in the actual production process, the laser cleaning parameters need to be slightly adjusted according to the specific laser cleaning effect.
[0070] The present invention completely removes the entire additional coating area through continuous laser cleaning by a laser etching machine. The coating on the surface of the pole piece will be converted into plasma under high-power laser etching, directly eliminating such irregular pattern areas that are prone to abnormal thickness thinning, excessive rolling and affecting the dynamic properties of the pole piece; improves the poor coating effect of the silicon negative electrode pole piece in the double-layer coating process, avoids the pole piece breakage phenomenon that may occur in the subsequent pole piece processing process, improves the quality and efficiency of the pole piece output, and thus ensures the performance and cycle stability of the lithium-ion battery prepared by the negative electrode pole piece.
[0071] The design capacity of the soft-pack battery cell is 4912 mAh, and the number of winding layers of the battery cell is 23. The preparation of the above-mentioned soft-pack battery cell is used as an example to further describe the technical solution in the present invention, but the embodiments of the present invention are not limited to this.
[0072] The current collector used for the negative electrode plate in the present invention includes but is not limited to copper foil, nickel foil, titanium foil and stainless steel foil; the current collector used for the positive electrode plate in the present invention includes but is not limited to aluminum foil, nickel foil, titanium foil and stainless steel foil; the active material used in the coating layer on the positive electrode plate includes but is not limited to LiCoO2, LiFePO4 and Li(Ni1-x-yCoxMny)O2.
[0073] Example 1
[0074] The carbon nanotube (CNT) material was coated on one side at a density of 2.5 g / m 2 Double-sided coating on a 5 μm thick bare copper foil to obtain a CNT-primed copper foil;
[0075] The length of CNT double-sided coating is shown in Figure 1 As shown, the CNT coating length of the long film surface is 1430.5 mm, the CNT coating length of the short film surface is 1316.0 mm, and the head empty foil length of the long film surface is 24.0 mm; the allowable error value in the coating process is ±1.5 mm;
[0076] At the same time, double-layer coating is performed on both sides of the CNT-coated copper foil. The coating layer structure is shown in Figure 2 As shown in the figure, the active material of the surface slurry is small-particle fast-filling graphite, and the active material of the bottom slurry is a mixture of large-particle high-density graphite and silicon-carbon material; the single-sided coating surface density of the surface small-particle fast-filling graphite is 19.5g / m 2 The single-sided coating density of the bottom layer of large-particle high-density graphite and silicon-carbon material mixture is 48.0g / m 2 ; The total coating surface density on the negative electrode sheet is 67.5g / m 2 ; The mass ratio of large-particle high-density graphite to silicon-carbon material in the bottom slurry is 92.57%:7.43%; The CNT-coated copper foil after double-layer coating is cut to obtain the negative electrode sheet to be laser-treated. The specific process parameters of the negative electrode sheet to be laser-treated are shown in Table 1;
[0077] The double-layer coating length of the negative electrode sheet to be laser treated is shown in Figure 3 As shown, the total length of the negative electrode sheet is 1454.5 mm, the total length of the coating area of the long film surface is 1436.5 mm, the total length of the coating area of the short film surface is 1322.0 mm, and the length of the additional coating area at the head and tail ends of the long film surface and the short film surface coating area is 10.0 mm; 3.0 mm length is reserved at both ends of the coating area for covering the CNT coating layer; the additional coating areas added at the head and tail of the long film surface and short film surface coating section of the negative electrode sheet to be laser treated are shown in FIG. Figure 4 , Figure 5As shown, the dotted areas on both sides are additional coating areas; the effect of abnormal patterns on the long film surface and short film surface of the negative electrode piece to be laser treated after double-layer coating is shown in Figure 6 , Figure 7 As shown;
[0078] A laser etching machine with a cleaning power of 600W, a pulse frequency of 400Hz, and a laser spot diameter of 0.05mm is used to perform a laser cleaning on the negative electrode sheet to be laser-treated to clean its surface coating;
[0079] After rewinding and unwinding the negative electrode sheet, the negative electrode sheet after the first cleaning is cleaned for a second time using the same laser etching machine with a cleaning power of 1400W, a pulse frequency of 400Hz, and a laser spot diameter of 0.05mm to clean its bottom coating;
[0080] The cleaning length of the primary laser cleaning and the secondary laser cleaning are both 10 mm and 71.8 mm in width; the cleaning width is equal to the width of the negative electrode sheet;
[0081] The negative electrode sheet after laser cleaning is cut to cut off the excess length generated during the cleaning process, that is, the area where the extra coating area at the tail of the negative electrode sheet is exposed after laser cleaning. Figure 8 , Fig. 9 As shown; finally, the negative electrode sheet is obtained, and the length of the coating layer on the negative electrode sheet is shown Fig.10 As shown;
[0082] The obtained negative electrode sheet is rolled and sheeted to obtain a wound negative electrode sheet;
[0083] The LiCoO2 active material was coated on one side at a density of 150.5 g / m 2 The double-sided single-layer coating was applied on an aluminum foil with a thickness of 8 μm to obtain a positive electrode sheet. The specific process parameters of the positive electrode sheet are shown in Table 2; the double-layer coating length of the positive electrode sheet is shown in Table 2. Fig.11 As shown, the total length of the positive electrode sheet is 1434.0 mm, the total length of the coating area of the short film surface is 1284.5 mm, and the total length of the coating area of the long film surface is 1409.0 mm;
[0084] The obtained positive electrode sheet is rolled, cut and sliced to obtain a wound positive electrode sheet; the above positive and negative electrode sheets and separators are wound to obtain a bare battery cell, and the wound bare battery cell is packaged, baked, injected, formed, double-sealed, and capacity divided to obtain a soft-pack lithium-ion battery.
[0085] Table 1. Process parameters of negative electrode sheets to be laser cleaned
[0086]
[0087] Table 2. Process parameters of positive electrode sheet
[0088]
[0089] Comparative Example 1
[0090] The CNT-primed copper foil was prepared according to the operating steps in Example 1; wherein the length of the CNT double-sided coating is shown in FIG. Fig.12 As shown, the CNT coating length of the long film surface is 1410.5 mm, the CNT coating length of the short film surface is 1296.0 mm, and the head empty foil length of the long film surface is 24.0 mm; the allowable error value in the coating process is ±1.5 mm;
[0091] According to the process parameters in Table 3, the steps of Example 1 were repeated to double-coat both sides of the CNT-primed copper foil and cut to obtain a negative electrode sheet. The double-coated length of the negative electrode sheet is shown in FIG. Fig.13 As shown, the total length of the negative electrode plate is 1434.5 mm, the total length of the coating area of the long film surface is 1416.5 mm, and the total length of the coating area of the short film surface is 1302.0 mm; compared with Example 1, the negative electrode plate in this comparative example 1 is not provided with an additional coating area, and is not subjected to laser cleaning treatment;
[0092] According to Table 2 in Example 1, Fig.11 Repeat the steps of Example 1 with the parameters in to prepare a positive electrode sheet;
[0093] The obtained positive electrode sheet is rolled, slit and sliced to obtain a wound positive electrode sheet;
[0094] The positive and negative electrode sheets and the separator are wound to obtain a bare cell, and the wound bare cell is packaged, baked, injected, formed, re-sealed, and capacity divided to obtain a soft-pack lithium-ion battery.
[0095] Table 3. Parameters of negative electrode processing without laser cleaning
[0096]
[0097] Test Case
[0098] The lithium ion batteries prepared in Example 1 and Comparative Example 1 were subjected to a step-down cycle at room temperature to test their capacity retention rate and thickness expansion rate. The capacity retention rate test results are shown in Table 4, and the thickness expansion rate test results are shown in Table 5.
[0099] The test method for capacity retention is as follows:
[0100] At room temperature of 25±3℃, the charging mode for 1-100 cycles is: 15.6A CC to 4.30V, 12.4A CC to4.35V CV to 1.8C, 1.8C CC to 4.40V CV to 1.5C, 1.5C CC to 4.50V CV to1.2C, 1.2CCC to 4.58V CV to 0.28C;
[0101] 101-300 weeks charging mode: 15.6A CC to 4.27V, 12.4A CC to 4.32V CV to1.8C, 1.8C CC to 4.40V CV to 1.5C, 1.5C CC to 4.50V CV to 1.2C, 1.2CCC to 4.56V CV to0.28C;
[0102] 301-800 weeks charging mode: 15.6A CC to 4.27V, 12.4A CC to 4.32V CV to1.8C, 1.8C CC to 4.40V CV to1.5C, 1.5C CC to 4.50V CV to 1.2C, 1.2CCC to 4.55V CV to0.28C;
[0103] Among them, CC represents constant current charging, CV represents constant voltage charging, and C represents the charge and discharge capacity rate of the battery;
[0104] 1-800 cycle discharge mode: 0.7C DC to 3.0V;
[0105] Where DC means constant current discharge;
[0106] Capacity retention rate = weekly discharge capacity / initial discharge capacity*100%.
[0107] The thickness expansion rate test method is as follows:
[0108] After every 100 cycles, the battery cell is charged to 4.53V at a constant current and constant voltage of 0.5C, with a cut-off rate of 0.02C, and fully charged. The thickness of the lithium battery is measured using a 600g PPG thickness gauge.
[0109] Thickness expansion rate = full-charge thickness per 100 cycles / initial full-charge thickness*100%.
[0110] Table 4. Capacity retention test results
[0111] Week 100 200 300 400 500 600 700 800 Example 1 98.3% 96.4% 95.5% 91.1% 89.5% 88.7% 87.5% 86.9% Comparative Example 1 97.9% 94.2% 92.5% 87.6% 85.9% 83.1% 80.6% 78.5%
[0112] Table 5. Thickness expansion test results
[0113] Week Initial full charge 100 200 300 400 500 600 700 800 Example 1 2.3% 5.5% 6.7% 7.5% 8.6% 9.4% 9.9% 10.7% 11.2% Comparative Example 1 2.6% 7.9% 9.7% 12.3% 14.1% 15.9% 16.7% 17.4% 18.1%
[0114] Secondly, the capacity retention rate of Example 1 and Comparative Example 1 under reduced pressure cycle is compared. Fig.14 As shown, the thickness expansion rate comparison is shown in Fig.15 As shown; Analysis of the above data shows that the capacity retention rate and thickness expansion rate of the lithium ion battery obtained in Example 1 are better than those of the lithium ion battery obtained in Comparative Example 1; It can be seen that after using laser to clean the abnormal patterns at the head and tail of the negative electrode sheet material layer in the present invention, the capacity retention rate and thickness expansion rate of the lithium ion battery are significantly improved, thereby improving the quality of the electrode sheet in the lithium ion battery and improving the long-term cycle stability of the battery; In addition, after 800 cycles at room temperature, the lithium ion battery obtained in Example 1 has a negative electrode cycle interface with less obvious lithium deposition at the head and tail than the lithium ion battery obtained in Comparative Example 1, indicating that after the coating head and tail of the negative electrode sheet are cleaned by laser, the edge density of the negative electrode sheet is more uniform, and the sheet dynamics are also improved, further proving the superiority of the present invention's method of using laser cleaning to remove abnormal coating areas at the head and tail of the coating layer in double-layer coating.
[0115] The above are only partial or preferred embodiments of the present invention. Neither the text nor the drawings can limit the scope of protection of the present invention. All equivalent structural changes made by using the contents of the present invention specification and drawings under the overall concept of the present invention, or direct / indirect application in other related technical fields are included in the scope of protection of the present invention.
Claims
1. A method for preparing a negative electrode sheet with improved double-layer coating abnormality, It is characterized in that The following steps are involved: Double-layer coating is performed on both sides of the negative electrode current collector, wherein the coating areas on both sides of the negative electrode current collector include an effective coating area and two additional coating areas respectively located at the head and tail ends of the effective coating area; The additional coating area is laser cleaned by using a laser etching machine to expose the surface of the negative electrode current collector to obtain a negative electrode plate.
2. The method for preparing a negative electrode sheet with improved double-layer coating abnormality according to claim 1, It is characterized in that The step of using a laser etching machine to laser clean the additional coating area to expose the surface of the negative electrode current collector to obtain the negative electrode plate includes: Cleaning the surface coating of the additional coating area once with a laser etching machine, and rolling up the negative electrode current collector after the cleaning is completed; Unwinding the negative electrode current collector, and performing secondary cleaning on the bottom coating of the additional coating area using a laser etching machine; The cleaned additional coating area located at the tail of the coating area on the negative electrode current collector is cut off to obtain a negative electrode plate.
3. The method for preparing a negative electrode sheet with improved double-layer coating abnormality according to claim 2, It is characterized in that The total laser cleaning depth of the additional coating area by the laser etcher is greater than the total thickness of the surface coating and the bottom coating.
4. The method for preparing a negative electrode sheet with improved double-layer coating abnormality according to claim 3, It is characterized in that The area of the laser cleaning is equal to the area of the additional coating area; the length of the additional coating area is 3-15 mm, and the width of the additional coating area is equal to the width of the effective coating area.
5. The method for preparing a negative electrode sheet with improved double-layer coating abnormality according to claim 4, It is characterized in that The mass ratio of the active substance in the bottom coating layer to the active substance in the top coating layer is 60-85%:15-40%; The active material used in the bottom coating is a mixture of large-particle high-density graphite and silicon-carbon material, and the active material used in the surface coating is small-particle fast-filling graphite; The mass ratio of the large-particle high-density graphite to the silicon-carbon material in the mixture of the large-particle high-density graphite and the silicon-carbon material is 75-95%:5-25%; The single-sided surface density of the bottom coating is ≥36g / m 2 ; The single-sided surface density of the surface coating is ≥13g / m 2 .
6. A method for preparing a negative electrode sheet with improved double-layer coating abnormality according to any one of claims 1 to 5, It is characterized in that The laser power of the first cleaning is 300-1000W; the laser power of the second cleaning is 800-3000W; the diameter of the laser spot used in the laser cleaning is 0.02-1.0mm; the laser pulse frequency used in the laser cleaning is 0.1-800Hz.
7. The method for preparing a negative electrode sheet with improved double-layer coating abnormality according to claim 6, It is characterized in that The two sides of the negative electrode current collector include a long film surface and a short film surface; the length of the effective coating area of the short film surface is smaller than the length of the effective coating area of the long film surface, and the tail of the effective coating area of the short film surface is aligned with the tail of the effective coating area of the long film surface; the lengths of the two additional coating areas at the head and tail of the coating area of the short film surface are equal to the lengths of the two additional coating areas at the head and tail of the coating area of the long film surface.
8. The method for preparing a negative electrode sheet with improved double-layer coating abnormality according to claim 7, It is characterized in that In the one cleaning, the laser cleaning power at the tail of the short film coating area is P 1 The laser cleaning power at the head of the short film coating area is P 2 The laser cleaning power at the tail of the long film coating area is P 3 The laser cleaning power at the head of the long film coating area is P 4 ; Among them, P 1 =P 2 =P 3 =P 4 ; In the secondary cleaning, the laser cleaning power at the tail of the short film coating area is P 5 The laser cleaning power at the head of the short film coating area is P 6 The laser cleaning power at the tail of the long film coating area is P 7 The laser cleaning power at the head of the long film coating area is P 8 ; Among them, P 5 =P 6 =P 7 =P 8 ; The laser spot diameter used for the tail laser cleaning of the short film surface coating area is D 1 The laser spot diameter used for the head laser cleaning of the short film surface coating area is D 2 The laser spot diameter used for the tail laser cleaning of the long film coating area is D 3 The laser spot diameter used for the head laser cleaning of the long film surface coating area is D 4 ; Among them, D 1 =D 2 =D 3 =D 4 ; The pulse frequency used for the tail laser cleaning of the short film surface coating area is f 1 The pulse frequency used for the laser cleaning of the head of the short film coating area is f 2 The pulse frequency used for the tail laser cleaning of the long film coating area is f 3 The pulse frequency used for the laser cleaning of the head of the long film coating area is f 4 ; Among them, f 1 =f 2 =f 3 =f 4 .
9. A negative electrode sheet, It is characterized in that The negative electrode plate is obtained by cleaning and removing the local areas at the head and tail of the double-layer coating by a laser etching machine.
10. A lithium ion battery, It is characterized in that It comprises a positive electrode sheet and the negative electrode sheet as claimed in claim 9.